NG5

Neutral filters exhibit almost constant attenuation inside the visible spectrum. They appear grey.
Find more information in the tabs below or on our website.
Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.
For customized filter products you can mark an article and use the request-button.
*product image is exemplary.
Spectral values guaranteed | |
---|---|
τi (405nm) | =0.56± 0,03 |
τi (546nm) | =0.57± 0,03 |
τi (694nm) | =0.62± 0,03 |
- SCHOTT
- NG5 - NG5
- Thickness
- 1.0
- Reflection factor
- 0.9231
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | 0.016 |
340 | 0.086 |
350 | 0.205 |
360 | 0.328 |
370 | 0.401 |
380 | 0.393 |
390 | 0.500 |
400 | 0.546 |
410 | 0.546 |
420 | 0.549 |
430 | 0.559 |
440 | 0.556 |
450 | 0.569 |
460 | 0.583 |
470 | 0.583 |
480 | 0.577 |
490 | 0.571 |
λ [nm] | |
---|---|
500 | 0.568 |
510 | 0.567 |
520 | 0.568 |
530 | 0.572 |
540 | 0.576 |
550 | 0.577 |
560 | 0.575 |
570 | 0.568 |
580 | 0.561 |
590 | 0.555 |
600 | 0.555 |
610 | 0.558 |
620 | 0.560 |
630 | 0.560 |
640 | 0.558 |
650 | 0.556 |
660 | 0.558 |
670 | 0.564 |
680 | 0.577 |
690 | 0.589 |
700 | 0.599 |
710 | 0.604 |
720 | 0.604 |
730 | 0.600 |
740 | 0.595 |
750 | 0.587 |
760 | 0.580 |
770 | 0.571 |
780 | 0.561 |
790 | 0.551 |
λ [nm] | |
---|---|
800 | 0.542 |
810 | 0.534 |
820 | 0.523 |
830 | 0.514 |
840 | 0.505 |
850 | 0.495 |
860 | 0.486 |
870 | 0.480 |
880 | 0.473 |
890 | 0.464 |
900 | 0.458 |
910 | 0.449 |
920 | 0.442 |
930 | 0.436 |
940 | 0.429 |
950 | 0.422 |
960 | 0.417 |
970 | 0.410 |
980 | 0.405 |
990 | 0.402 |
1,000 | 0.397 |
1,010 | 0.394 |
1,020 | 0.390 |
1,030 | 0.387 |
1,040 | 0.385 |
1,050 | 0.383 |
1,060 | 0.380 |
1,070 | 0.379 |
1,080 | 0.377 |
1,090 | 0.376 |
λ [nm] | |
---|---|
1,100 | 0.379 |
1,110 | 0.381 |
1,120 | 0.381 |
1,130 | 0.382 |
1,140 | 0.382 |
1,150 | 0.383 |
1,160 | 0.383 |
1,170 | 0.384 |
1,180 | 0.386 |
1,190 | 0.388 |
1,200 | 0.390 |
1,250 | 0.407 |
1,300 | 0.440 |
1,350 | 0.468 |
1,400 | 0.500 |
1,450 | 0.532 |
1,500 | 0.560 |
1,550 | 0.576 |
1,600 | 0.586 |
1,650 | 0.590 |
1,700 | 0.590 |
1,750 | 0.593 |
1,800 | 0.595 |
1,850 | 0.600 |
1,900 | 0.610 |
1,950 | 0.619 |
2,000 | 0.630 |
2,050 | 0.641 |
2,100 | 0.650 |
2,150 | 0.657 |
λ [nm] | |
---|---|
2,200 | 0.662 |
2,250 | 0.671 |
2,300 | 0.680 |
2,350 | 0.688 |
2,400 | 0.690 |
2,450 | 0.695 |
2,500 | 0.700 |
2,550 | 0.702 |
2,600 | 0.704 |
2,650 | 0.700 |
2,700 | 0.660 |
2,750 | 0.311 |
2,800 | 0.170 |
2,850 | 0.158 |
2,900 | 0.170 |
2,950 | 0.194 |
3,000 | 0.220 |
3,050 | 0.248 |
3,100 | 0.280 |
3,150 | 0.306 |
3,200 | 0.336 |
3,250 | 0.363 |
3,300 | 0.370 |
3,350 | 0.351 |
3,400 | 0.290 |
3,450 | 0.217 |
3,500 | 0.150 |
3,550 | 0.101 |
3,600 | 0.070 |
3,650 | 0.059 |
λ [nm] | |
---|---|
3,700 | 0.071 |
3,750 | 0.108 |
3,800 | 0.140 |
3,850 | 0.158 |
3,900 | 0.147 |
3,950 | 0.118 |
4,000 | 0.100 |
4,050 | 0.089 |
4,100 | 0.095 |
4,150 | 0.100 |
4,200 | 0.100 |
4,250 | 0.094 |
4,300 | 0.078 |
4,350 | 0.055 |
4,400 | 0.040 |
4,450 | 0.025 |
4,500 | 0.016 |
4,550 | 0.010 |
4,600 | 0.006 |
4,650 | 0.003 |
4,700 | 0.002 |
4,750 | 0.001 |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
Reflection factor | |
---|---|
Pd | 0.923 |
Reference thickness | |
---|---|
d [mm] | 1 |
Spectral values guaranteed | |
---|---|
τi (405nm) | =0.56± 0,03 |
τi (546nm) | =0.57± 0,03 |
τi (694nm) | =0.62± 0,03 |
Refractive Indices n |
---|
nd (587.6 nm) = 1.500 |
Colorimetric evaluation
Illuminant | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Illuminant | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Illuminant | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
Density | |
---|---|
p [g/cm3] | 2.43 |
Bubble content | |
---|---|
Bubble class | 2 |
Transformation temperature | |
---|---|
Tg [°C] | 474 |
Temperature coefficient | |
---|---|
Tk [nm/°C] |
Chemical Resistance | |
---|---|
FR class | 1 |
SR class | 3.2 |
AR class | 2.0 |
Thermal expansion | |
---|---|
α-30°C/+70°C [10-6/K] | 6.6 |
α20°C/300°C [10-6/K] | 7.3 |
α20°C/200°C [10-6/K] |