NG11

玻璃类型 |
物品编号 |
长度 |
宽度 |
厚度 |
重量 |
---|
- SCHOTT
- NG11 - NG11
- 厚度
- 1.0
- 反射系数
- 0.9234
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | 0.007 |
330 | 0.074 |
340 | 0.239 |
350 | 0.424 |
360 | 0.567 |
370 | 0.629 |
380 | 0.597 |
390 | 0.717 |
400 | 0.753 |
410 | 0.748 |
420 | 0.747 |
430 | 0.754 |
440 | 0.752 |
450 | 0.756 |
460 | 0.779 |
470 | 0.779 |
480 | 0.777 |
490 | 0.775 |
λ [nm] | |
---|---|
500 | 0.772 |
510 | 0.773 |
520 | 0.777 |
530 | 0.781 |
540 | 0.784 |
550 | 0.783 |
560 | 0.782 |
570 | 0.777 |
580 | 0.773 |
590 | 0.770 |
600 | 0.771 |
610 | 0.772 |
620 | 0.772 |
630 | 0.771 |
640 | 0.769 |
650 | 0.768 |
660 | 0.769 |
670 | 0.774 |
680 | 0.781 |
690 | 0.789 |
700 | 0.792 |
710 | 0.793 |
720 | 0.791 |
730 | 0.786 |
740 | 0.782 |
750 | 0.776 |
760 | 0.770 |
770 | 0.765 |
780 | 0.758 |
790 | 0.751 |
λ [nm] | |
---|---|
800 | 0.744 |
810 | 0.738 |
820 | 0.730 |
830 | 0.722 |
840 | 0.717 |
850 | 0.709 |
860 | 0.703 |
870 | 0.694 |
880 | 0.685 |
890 | 0.681 |
900 | 0.675 |
910 | 0.670 |
920 | 0.664 |
930 | 0.660 |
940 | 0.655 |
950 | 0.652 |
960 | 0.645 |
970 | 0.643 |
980 | 0.639 |
990 | 0.636 |
1,000 | 0.633 |
1,010 | 0.631 |
1,020 | 0.628 |
1,030 | 0.626 |
1,040 | 0.624 |
1,050 | 0.624 |
1,060 | 0.623 |
1,070 | 0.622 |
1,080 | 0.621 |
1,090 | 0.622 |
λ [nm] | |
---|---|
1,100 | 0.624 |
1,110 | 0.625 |
1,120 | 0.627 |
1,130 | 0.628 |
1,140 | 0.629 |
1,150 | 0.630 |
1,160 | 0.632 |
1,170 | 0.633 |
1,180 | 0.635 |
1,190 | 0.637 |
1,200 | 0.640 |
1,250 | 0.662 |
1,300 | 0.680 |
1,350 | 0.703 |
1,400 | 0.729 |
1,450 | 0.747 |
1,500 | 0.769 |
1,550 | 0.779 |
1,600 | 0.784 |
1,650 | 0.784 |
1,700 | 0.783 |
1,750 | 0.783 |
1,800 | 0.783 |
1,850 | 0.784 |
1,900 | 0.790 |
1,950 | 0.793 |
2,000 | 0.800 |
2,050 | 0.806 |
2,100 | 0.810 |
2,150 | 0.810 |
λ [nm] | |
---|---|
2,200 | 0.810 |
2,250 | 0.812 |
2,300 | 0.820 |
2,350 | 0.823 |
2,400 | 0.820 |
2,450 | 0.820 |
2,500 | 0.820 |
2,550 | 0.820 |
2,600 | 0.820 |
2,650 | 0.813 |
2,700 | 0.740 |
2,750 | 0.255 |
2,800 | 0.120 |
2,850 | 0.115 |
2,900 | 0.130 |
2,950 | 0.153 |
3,000 | 0.176 |
3,050 | 0.207 |
3,100 | 0.240 |
3,150 | 0.275 |
3,200 | 0.309 |
3,250 | 0.342 |
3,300 | 0.352 |
3,350 | 0.341 |
3,400 | 0.290 |
3,450 | 0.219 |
3,500 | 0.150 |
3,550 | 0.102 |
3,600 | 0.074 |
3,650 | 0.063 |
λ [nm] | |
---|---|
3,700 | 0.080 |
3,750 | 0.116 |
3,800 | 0.158 |
3,850 | 0.172 |
3,900 | 0.157 |
3,950 | 0.130 |
4,000 | 0.106 |
4,050 | 0.106 |
4,100 | 0.106 |
4,150 | 0.112 |
4,200 | 0.116 |
4,250 | 0.107 |
4,300 | 0.087 |
4,350 | 0.060 |
4,400 | 0.042 |
4,450 | 0.029 |
4,500 | 0.017 |
4,550 | 0.010 |
4,600 | 0.006 |
4,650 | 0.003 |
4,700 | 0.002 |
4,750 | 0.001 |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.923 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (405nm) | =0.76± 0,02 |
τi (546nm) | =0.77± 0,02 |
τi (694nm) | =0.79± 0,02 |
折射率 n |
---|
nF (486.1 nm) = 1.504 |
nh (404.7 nm) = 1.512 |
ng (435.8 nm) = 1.508 |
ns (852.1 nm) = 1.492 |
ne (546.1 nm) = 1.500 |
nd (587.6 nm) = 1.499 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.4098 |
气泡含量 | |
---|---|
气泡等级 | 2 |
玻转温度 | |
---|---|
Tg [°C] | 481 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 1 |
耐酸性 | 3.4 |
耐碱性 | 2.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 6.67 |
α20°C/300°C [10-6/K] | 7.2 |
α20°C/200°C [10-6/K] | 7 |