UG5

玻璃类型 |
物品编号 |
长度 |
宽度 |
厚度 |
重量 |
---|
- SCHOTT
- UG5 - UG5
- 厚度
- 1.0
- 反射系数
- 0.9135
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | 0.069 |
230 | 0.450 |
240 | 0.718 |
250 | 0.826 |
260 | 0.879 |
270 | 0.912 |
280 | 0.939 |
290 | 0.952 |
300 | 0.960 |
310 | 0.966 |
320 | 0.976 |
330 | 0.980 |
340 | 0.982 |
350 | 0.981 |
360 | 0.976 |
370 | 0.960 |
380 | 0.912 |
390 | 0.787 |
400 | 0.570 |
410 | 0.360 |
420 | 0.236 |
430 | 0.178 |
440 | 0.168 |
450 | 0.178 |
460 | 0.183 |
470 | 0.166 |
480 | 0.147 |
490 | 0.126 |
λ [nm] | |
---|---|
500 | 0.095 |
510 | 0.070 |
520 | 0.046 |
530 | 0.033 |
540 | 0.030 |
550 | 0.030 |
560 | 0.022 |
570 | 0.011 |
580 | 0.008 |
590 | 0.009 |
600 | 0.012 |
610 | 0.015 |
620 | 0.017 |
630 | 0.023 |
640 | 0.044 |
650 | 0.101 |
660 | 0.227 |
670 | 0.414 |
680 | 0.595 |
690 | 0.727 |
700 | 0.799 |
710 | 0.829 |
720 | 0.832 |
730 | 0.818 |
740 | 0.795 |
750 | 0.769 |
760 | 0.743 |
770 | 0.719 |
780 | 0.698 |
790 | 0.679 |
λ [nm] | |
---|---|
800 | 0.665 |
810 | 0.655 |
820 | 0.648 |
830 | 0.644 |
840 | 0.642 |
850 | 0.644 |
860 | 0.646 |
870 | 0.648 |
880 | 0.649 |
890 | 0.652 |
900 | 0.654 |
910 | 0.661 |
920 | 0.663 |
930 | 0.669 |
940 | 0.675 |
950 | 0.683 |
960 | 0.688 |
970 | 0.696 |
980 | 0.703 |
990 | 0.711 |
1,000 | 0.716 |
1,010 | 0.723 |
1,020 | 0.728 |
1,030 | 0.732 |
1,040 | 0.734 |
1,050 | 0.734 |
1,060 | 0.735 |
1,070 | 0.731 |
1,080 | 0.727 |
1,090 | 0.719 |
λ [nm] | |
---|---|
1,100 | 0.712 |
1,110 | 0.696 |
1,120 | 0.683 |
1,130 | 0.672 |
1,140 | 0.662 |
1,150 | 0.644 |
1,160 | 0.625 |
1,170 | 0.612 |
1,180 | 0.595 |
1,190 | 0.576 |
1,200 | 0.560 |
1,250 | 0.489 |
1,300 | 0.443 |
1,350 | 0.435 |
1,400 | 0.440 |
1,450 | 0.437 |
1,500 | 0.434 |
1,550 | 0.437 |
1,600 | 0.456 |
1,650 | 0.477 |
1,700 | 0.490 |
1,750 | 0.498 |
1,800 | 0.500 |
1,850 | 0.513 |
1,900 | 0.529 |
1,950 | 0.553 |
2,000 | 0.570 |
2,050 | 0.587 |
2,100 | 0.600 |
2,150 | 0.609 |
λ [nm] | |
---|---|
2,200 | 0.604 |
2,250 | 0.599 |
2,300 | 0.596 |
2,350 | 0.600 |
2,400 | 0.600 |
2,450 | 0.597 |
2,500 | 0.584 |
2,550 | 0.525 |
2,600 | 0.501 |
2,650 | 0.481 |
2,700 | 0.446 |
2,750 | 0.353 |
2,800 | 0.120 |
2,850 | 0.036 |
2,900 | 0.014 |
2,950 | 0.007 |
3,000 | 0.004 |
3,050 | 0.002 |
3,100 | 0.001 |
3,150 | < 10⁻³ |
3,200 | < 10⁻³ |
3,250 | < 10⁻³ |
3,300 | < 10⁻³ |
3,350 | < 10⁻³ |
3,400 | < 10⁻³ |
3,450 | < 10⁻³ |
3,500 | < 10⁻³ |
3,550 | < 10⁻³ |
3,600 | < 10⁻³ |
3,650 | < 10⁻³ |
λ [nm] | |
---|---|
3,700 | < 10⁻³ |
3,750 | < 10⁻³ |
3,800 | < 10⁻³ |
3,850 | < 10⁻³ |
3,900 | < 10⁻³ |
3,950 | < 10⁻³ |
4,000 | < 10⁻³ |
4,050 | < 10⁻³ |
4,100 | < 10⁻³ |
4,150 | < 10⁻³ |
4,200 | < 10⁻³ |
4,250 | < 10⁻³ |
4,300 | < 10⁻³ |
4,350 | < 10⁻³ |
4,400 | < 10⁻³ |
4,450 | < 10⁻³ |
4,500 | < 10⁻³ |
4,550 | < 10⁻³ |
4,600 | < 10⁻³ |
4,650 | < 10⁻³ |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.914 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (254nm) | ≥0.8 |
τi (308nm) | ≥0.94 |
τi (405nm) | ≤0.5 |
τi (546nm) | ≤0.05 |
τi (633nm) | ≤0.05 |
τi (725nm) | ≤0.05 |
折射率 n |
---|
n (253.7 nm) = 1.600 |
nd (587.6 nm) = 1.540 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.85 |
气泡含量 | |
---|---|
气泡等级 |
玻转温度 | |
---|---|
Tg [°C] | 462 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 3.0 |
耐碱性 | 2.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 8.1 |
α20°C/300°C [10-6/K] | 9.4 |
α20°C/200°C [10-6/K] |