λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | 0.006 |
260 | 0.103 |
270 | 0.364 |
280 | 0.626 |
290 | 0.798 |
300 | 0.899 |
310 | 0.951 |
320 | 0.973 |
330 | 0.983 |
340 | 0.986 |
350 | 0.987 |
360 | 0.987 |
370 | 0.984 |
380 | 0.981 |
390 | 0.975 |
400 | 0.951 |
410 | 0.916 |
420 | 0.874 |
430 | 0.815 |
440 | 0.745 |
450 | 0.658 |
460 | 0.550 |
470 | 0.393 |
480 | 0.222 |
490 | 0.097 |
λ [nm] | |
---|---|
500 | 0.043 |
510 | 0.013 |
520 | 0.003 |
530 | < 10⁻³ |
540 | < 10⁻³ |
550 | < 10⁻³ |
560 | 0.002 |
570 | 0.001 |
580 | < 10⁻³ |
590 | < 10⁻³ |
600 | < 10⁻³ |
610 | < 10⁻³ |
620 | < 10⁻³ |
630 | < 10⁻³ |
640 | < 10⁻³ |
650 | < 10⁻³ |
660 | < 10⁻³ |
670 | < 10⁻³ |
680 | 0.010 |
690 | 0.100 |
700 | 0.359 |
710 | 0.655 |
720 | 0.846 |
730 | 0.938 |
740 | 0.976 |
750 | 0.986 |
760 | 0.988 |
770 | 0.989 |
780 | 0.990 |
790 | 0.990 |
λ [nm] | |
---|---|
800 | 0.990 |
810 | 0.990 |
820 | 0.990 |
830 | 0.990 |
840 | 0.989 |
850 | 0.989 |
860 | 0.989 |
870 | 0.989 |
880 | 0.988 |
890 | 0.988 |
900 | 0.988 |
910 | 0.987 |
920 | 0.986 |
930 | 0.984 |
940 | 0.981 |
950 | 0.976 |
960 | 0.971 |
970 | 0.965 |
980 | 0.957 |
990 | 0.948 |
1,000 | 0.937 |
1,010 | 0.923 |
1,020 | 0.910 |
1,030 | 0.891 |
1,040 | 0.868 |
1,050 | 0.843 |
1,060 | 0.813 |
1,070 | 0.780 |
1,080 | 0.746 |
1,090 | 0.706 |
λ [nm] | |
---|---|
1,100 | 0.667 |
1,110 | 0.615 |
1,120 | 0.568 |
1,130 | 0.525 |
1,140 | 0.480 |
1,150 | 0.432 |
1,160 | 0.388 |
1,170 | 0.343 |
1,180 | 0.308 |
1,190 | 0.273 |
1,200 | 0.241 |
1,250 | 0.146 |
1,300 | 0.120 |
1,350 | 0.141 |
1,400 | 0.150 |
1,450 | 0.118 |
1,500 | 0.100 |
1,550 | 0.100 |
1,600 | 0.124 |
1,650 | 0.141 |
1,700 | 0.140 |
1,750 | 0.133 |
1,800 | 0.144 |
1,850 | 0.185 |
1,900 | 0.250 |
1,950 | 0.328 |
2,000 | 0.400 |
2,050 | 0.462 |
2,100 | 0.520 |
2,150 | 0.567 |
λ [nm] | |
---|---|
2,200 | 0.620 |
2,250 | 0.657 |
2,300 | 0.701 |
2,350 | 0.735 |
2,400 | 0.754 |
2,450 | 0.764 |
2,500 | 0.765 |
2,550 | 0.761 |
2,600 | 0.756 |
2,650 | 0.743 |
2,700 | 0.724 |
2,750 | 0.644 |
2,800 | 0.587 |
2,850 | 0.576 |
2,900 | 0.572 |
2,950 | 0.570 |
3,000 | 0.562 |
3,050 | 0.548 |
3,100 | 0.526 |
3,150 | 0.507 |
3,200 | 0.484 |
3,250 | 0.463 |
3,300 | 0.444 |
3,350 | 0.427 |
3,400 | 0.410 |
3,450 | 0.398 |
3,500 | 0.392 |
3,550 | 0.390 |
3,600 | 0.392 |
3,650 | 0.398 |
λ [nm] | |
---|---|
3,700 | 0.404 |
3,750 | 0.413 |
3,800 | 0.423 |
3,850 | 0.433 |
3,900 | 0.446 |
3,950 | 0.456 |
4,000 | 0.460 |
4,050 | 0.456 |
4,100 | 0.440 |
4,150 | 0.417 |
4,200 | 0.392 |
4,250 | 0.367 |
4,300 | 0.337 |
4,350 | 0.292 |
4,400 | 0.250 |
4,450 | 0.200 |
4,500 | 0.160 |
4,550 | 0.113 |
4,600 | 0.078 |
4,650 | 0.056 |
4,700 | 0.042 |
4,750 | 0.035 |
4,800 | 0.032 |
4,850 | 0.031 |
4,900 | 0.027 |
4,950 | 0.020 |
5,000 | 0.011 |
5,050 | 0.005 |
5,100 | 0.002 |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.921 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (365nm) | ≥0.94 |
τi (633nm) | ≤0.00005 |
折射率 n |
---|
nF (486.1 nm) = 1.516 |
ng (435.8 nm) = 1.520 |
ns (852.1 nm) = 1.502 |
ne (546.1 nm) = 1.512 |
nd (587.6 nm) = 1.510 |
n (302.1 nm) = 1.548 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.160 | 0.166 | 0.170 |
y | 0.042 | 0.024 | 0.020 |
Y | 1 | 0 | 0 |
λd [nm] | 458 | 447 | 440 |
Pe | 0.96 | 0.98 | 0.98 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.157 | 0.163 | 0.167 |
y | 0.038 | 0.022 | 0.018 |
Y | 1 | 0 | 0 |
λd [nm] | 457 | 447 | 442 |
Pe | 0.97 | 0.98 | 0.99 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.154 | 0.160 | 0.163 |
y | 0.029 | 0.018 | 0.014 |
Y | 2 | 1 | 0 |
λd [nm] | 455 | 448 | 444 |
Pe | 0.98 | 0.99 | 1.00 |
密度 | |
---|---|
p [g/cm3] | 2.56 |
气泡含量 | |
---|---|
气泡等级 |
玻转温度 | |
---|---|
Tg [°C] | 478 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 1.0 |
耐碱性 | 1.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 8.8 |
α20°C/300°C [10-6/K] | 10.2 |
α20°C/200°C [10-6/K] |