RG715

- SCHOTT
- RG715 - RG715
- 厚度
- 3.0
- 反射系数
- 0.0000
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | < 10⁻³ |
340 | < 10⁻³ |
350 | < 10⁻³ |
360 | < 10⁻³ |
370 | < 10⁻³ |
380 | < 10⁻³ |
390 | < 10⁻³ |
400 | < 10⁻³ |
410 | < 10⁻³ |
420 | < 10⁻³ |
430 | < 10⁻³ |
440 | < 10⁻³ |
450 | < 10⁻³ |
460 | < 10⁻³ |
470 | < 10⁻³ |
480 | < 10⁻³ |
490 | < 10⁻³ |
λ [nm] | |
---|---|
500 | < 10⁻³ |
510 | < 10⁻³ |
520 | < 10⁻³ |
530 | < 10⁻³ |
540 | < 10⁻³ |
550 | < 10⁻³ |
560 | < 10⁻³ |
570 | < 10⁻³ |
580 | < 10⁻³ |
590 | < 10⁻³ |
600 | < 10⁻³ |
610 | < 10⁻³ |
620 | < 10⁻³ |
630 | < 10⁻³ |
640 | < 10⁻³ |
650 | < 10⁻³ |
660 | < 10⁻³ |
670 | < 10⁻³ |
680 | < 10⁻³ |
690 | 0.005 |
700 | 0.059 |
710 | 0.311 |
720 | 0.666 |
730 | 0.866 |
740 | 0.941 |
750 | 0.967 |
760 | 0.976 |
770 | 0.979 |
780 | 0.980 |
790 | 0.981 |
λ [nm] | |
---|---|
800 | 0.980 |
810 | 0.980 |
820 | 0.980 |
830 | 0.980 |
840 | 0.980 |
850 | 0.980 |
860 | 0.979 |
870 | 0.979 |
880 | 0.979 |
890 | 0.980 |
900 | 0.980 |
910 | 0.980 |
920 | 0.980 |
930 | 0.980 |
940 | 0.980 |
950 | 0.980 |
960 | 0.980 |
970 | 0.980 |
980 | 0.980 |
990 | 0.981 |
1,000 | 0.981 |
1,010 | 0.981 |
1,020 | 0.981 |
1,030 | 0.981 |
1,040 | 0.981 |
1,050 | 0.981 |
1,060 | 0.981 |
1,070 | 0.981 |
1,080 | 0.982 |
1,090 | 0.982 |
λ [nm] | |
---|---|
1,100 | 0.982 |
1,110 | 0.982 |
1,120 | 0.982 |
1,130 | 0.982 |
1,140 | 0.982 |
1,150 | 0.983 |
1,160 | 0.983 |
1,170 | 0.983 |
1,180 | 0.983 |
1,190 | 0.983 |
1,200 | 0.984 |
1,250 | 0.985 |
1,300 | 0.986 |
1,350 | 0.988 |
1,400 | 0.988 |
1,450 | 0.990 |
1,500 | 0.992 |
1,550 | 0.993 |
1,600 | 0.993 |
1,650 | 0.993 |
1,700 | 0.992 |
1,750 | 0.990 |
1,800 | 0.989 |
1,850 | 0.988 |
1,900 | 0.987 |
1,950 | 0.987 |
2,000 | 0.986 |
2,050 | 0.985 |
2,100 | 0.984 |
2,150 | 0.980 |
λ [nm] | |
---|---|
2,200 | 0.968 |
2,250 | 0.964 |
2,300 | 0.968 |
2,350 | 0.968 |
2,400 | 0.966 |
2,450 | 0.960 |
2,500 | 0.954 |
2,550 | 0.959 |
2,600 | 0.960 |
2,650 | 0.949 |
2,700 | 0.902 |
2,750 | 0.560 |
2,800 | 0.365 |
2,850 | 0.338 |
2,900 | 0.336 |
2,950 | 0.334 |
3,000 | 0.324 |
3,050 | 0.307 |
3,100 | 0.286 |
3,150 | 0.266 |
3,200 | 0.248 |
3,250 | 0.233 |
3,300 | 0.220 |
3,350 | 0.212 |
3,400 | 0.207 |
3,450 | 0.209 |
3,500 | 0.217 |
3,550 | 0.231 |
3,600 | 0.248 |
3,650 | 0.265 |
λ [nm] | |
---|---|
3,700 | 0.283 |
3,750 | 0.299 |
3,800 | 0.313 |
3,850 | 0.323 |
3,900 | 0.330 |
3,950 | 0.330 |
4,000 | 0.325 |
4,050 | 0.315 |
4,100 | 0.299 |
4,150 | 0.276 |
4,200 | 0.246 |
4,250 | 0.212 |
4,300 | 0.167 |
4,350 | 0.124 |
4,400 | 0.080 |
4,450 | 0.044 |
4,500 | 0.020 |
4,550 | 0.008 |
4,600 | 0.003 |
4,650 | 0.001 |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.000 |
参考厚度 | |
---|---|
d [mm] | 3 |
承诺光谱值 | |
---|---|
λs (τi = 0.00001) [nm] | 620 |
λc (τi = 0.5) [nm] | 715 ± 9 |
λp1 (τi = 0.92) [nm] | 810 |
折射率 n |
---|
ns (852.1 nm) = 1.530 |
ne (546.1 nm) = 1.540 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.76 |
气泡含量 | |
---|---|
气泡等级 | 3 |
玻转温度 | |
---|---|
Tg [°C] | 532 |
温度系数 | |
---|---|
Tk [nm/°C] | 0.18 |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 1.0 |
耐碱性 | 1.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 8.1 |
α20°C/300°C [10-6/K] | 9.4 |
α20°C/200°C [10-6/K] |