RG850

- SCHOTT
- RG850 - RG850
- 厚度
- 3.0
- 反射系数
- 0.9087
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | < 10⁻³ |
340 | < 10⁻³ |
350 | < 10⁻³ |
360 | < 10⁻³ |
370 | < 10⁻³ |
380 | < 10⁻³ |
390 | < 10⁻³ |
400 | < 10⁻³ |
410 | < 10⁻³ |
420 | < 10⁻³ |
430 | < 10⁻³ |
440 | < 10⁻³ |
450 | < 10⁻³ |
460 | < 10⁻³ |
470 | < 10⁻³ |
480 | < 10⁻³ |
490 | < 10⁻³ |
λ [nm] | |
---|---|
500 | < 10⁻³ |
510 | < 10⁻³ |
520 | < 10⁻³ |
530 | < 10⁻³ |
540 | < 10⁻³ |
550 | < 10⁻³ |
560 | < 10⁻³ |
570 | < 10⁻³ |
580 | < 10⁻³ |
590 | < 10⁻³ |
600 | < 10⁻³ |
610 | < 10⁻³ |
620 | < 10⁻³ |
630 | < 10⁻³ |
640 | < 10⁻³ |
650 | < 10⁻³ |
660 | < 10⁻³ |
670 | < 10⁻³ |
680 | < 10⁻³ |
690 | < 10⁻³ |
700 | < 10⁻³ |
710 | < 10⁻³ |
720 | < 10⁻³ |
730 | < 10⁻³ |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | < 10⁻³ |
790 | < 10⁻³ |
λ [nm] | |
---|---|
800 | 0.001 |
810 | 0.005 |
820 | 0.024 |
830 | 0.091 |
840 | 0.261 |
850 | 0.500 |
860 | 0.704 |
870 | 0.838 |
880 | 0.905 |
890 | 0.940 |
900 | 0.957 |
910 | 0.965 |
920 | 0.971 |
930 | 0.974 |
940 | 0.977 |
950 | 0.978 |
960 | 0.979 |
970 | 0.980 |
980 | 0.981 |
990 | 0.982 |
1,000 | 0.983 |
1,010 | 0.984 |
1,020 | 0.985 |
1,030 | 0.986 |
1,040 | 0.987 |
1,050 | 0.987 |
1,060 | 0.988 |
1,070 | 0.989 |
1,080 | 0.989 |
1,090 | 0.990 |
λ [nm] | |
---|---|
1,100 | 0.990 |
1,110 | 0.991 |
1,120 | 0.991 |
1,130 | 0.992 |
1,140 | 0.992 |
1,150 | 0.993 |
1,160 | 0.993 |
1,170 | 0.994 |
1,180 | 0.994 |
1,190 | 0.994 |
1,200 | 0.995 |
1,250 | 0.996 |
1,300 | 0.997 |
1,350 | 0.998 |
1,400 | 0.997 |
1,450 | 0.998 |
1,500 | 1.000 |
1,550 | 1.000 |
1,600 | 1.000 |
1,650 | 0.999 |
1,700 | 0.997 |
1,750 | 0.995 |
1,800 | 0.993 |
1,850 | 0.992 |
1,900 | 0.991 |
1,950 | 0.989 |
2,000 | 0.987 |
2,050 | 0.987 |
2,100 | 0.984 |
2,150 | 0.978 |
λ [nm] | |
---|---|
2,200 | 0.966 |
2,250 | 0.957 |
2,300 | 0.958 |
2,350 | 0.956 |
2,400 | 0.947 |
2,450 | 0.941 |
2,500 | 0.937 |
2,550 | 0.934 |
2,600 | 0.927 |
2,650 | 0.911 |
2,700 | 0.865 |
2,750 | 0.510 |
2,800 | 0.224 |
2,850 | 0.169 |
2,900 | 0.142 |
2,950 | 0.121 |
3,000 | 0.104 |
3,050 | 0.093 |
3,100 | 0.083 |
3,150 | 0.077 |
3,200 | 0.074 |
3,250 | 0.072 |
3,300 | 0.068 |
3,350 | 0.064 |
3,400 | 0.059 |
3,450 | 0.054 |
3,500 | 0.049 |
3,550 | 0.045 |
3,600 | 0.045 |
3,650 | 0.045 |
λ [nm] | |
---|---|
3,700 | 0.042 |
3,750 | 0.037 |
3,800 | 0.035 |
3,850 | 0.042 |
3,900 | 0.055 |
3,950 | 0.072 |
4,000 | 0.071 |
4,050 | 0.063 |
4,100 | 0.057 |
4,150 | 0.052 |
4,200 | 0.049 |
4,250 | 0.052 |
4,300 | 0.051 |
4,350 | 0.044 |
4,400 | 0.033 |
4,450 | 0.023 |
4,500 | 0.013 |
4,550 | 0.007 |
4,600 | 0.003 |
4,650 | 0.001 |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.909 |
参考厚度 | |
---|---|
d [mm] | 3 |
承诺光谱值 | |
---|---|
λs (τi = 0.00001) [nm] | 700 |
λc (τi = 0.5) [nm] | 850 ± 9 |
λp1 (τi = 0.92) [nm] | 950 |
λp2 (τi = 0.97) [nm] | 1200 |
折射率 n |
---|
ns (852.1 nm) = 1.550 |
nd (587.6 nm) = 1.560 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.93 |
气泡含量 | |
---|---|
气泡等级 | 3 |
玻转温度 | |
---|---|
Tg [°C] | 554 |
温度系数 | |
---|---|
Tk [nm/°C] | 0.24 |
耐化学性 | |
---|---|
耐污性 | 5 |
耐酸性 | 53.4 |
耐碱性 | 1.3 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 9.5 |
α20°C/300°C [10-6/K] | 10.5 |
α20°C/200°C [10-6/K] |