BG18

Longpass filters provide cut-on wavelengths in the ultra-violet (UV), visible, or near-infrared (NIR) spectra. The color glass substrates feature high spectral transmittance within their wavelength ranges. .

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

BG18
Spectral values guaranteed
τi (350nm) ≥ 0,3
τi (405nm) ≥ 0,65
τi (514nm) ≥ 0,88
τi (633nm) ≤ 0,25
τi (694nm) ≤ 0,03
τi (1060nm) ≤ 0,0005
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
BG18 - BG18
Thickness
1.0
Reflection factor
0.9150
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 0.033
330 0.156
340 0.305
350 0.416
360 0.497
370 0.552
380 0.603
390 0.643
400 0.682
410 0.719
420 0.751
430 0.780
440 0.806
450 0.830
460 0.853
470 0.872
480 0.885
490 0.899
λ [nm]
500 0.911
510 0.916
520 0.915
530 0.908
540 0.892
550 0.863
560 0.819
570 0.761
580 0.686
590 0.600
600 0.506
610 0.411
620 0.322
630 0.242
640 0.175
650 0.122
660 0.082
670 0.053
680 0.033
690 0.020
700 0.012
710 0.007
720 0.004
730 0.002
740 0.001
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 < 10⁻³
840 < 10⁻³
850 < 10⁻³
860 < 10⁻³
870 < 10⁻³
880 < 10⁻³
890 < 10⁻³
900 < 10⁻³
910 < 10⁻³
920 < 10⁻³
930 < 10⁻³
940 < 10⁻³
950 < 10⁻³
960 < 10⁻³
970 < 10⁻³
980 < 10⁻³
990 < 10⁻³
1,000 < 10⁻³
1,010 < 10⁻³
1,020 < 10⁻³
1,030 < 10⁻³
1,040 < 10⁻³
1,050 < 10⁻³
1,060 < 10⁻³
1,070 < 10⁻³
1,080 < 10⁻³
1,090 < 10⁻³
λ [nm]
1,100 < 10⁻³
1,110 < 10⁻³
1,120 < 10⁻³
1,130 < 10⁻³
1,140 0.001
1,150 0.001
1,160 0.002
1,170 0.002
1,180 0.002
1,190 0.003
1,200 0.003
1,250 0.007
1,300 0.018
1,350 0.033
1,400 0.060
1,450 0.096
1,500 0.150
1,550 0.214
1,600 0.280
1,650 0.359
1,700 0.436
1,750 0.502
1,800 0.560
1,850 0.619
1,900 0.660
1,950 0.707
2,000 0.743
2,050 0.763
2,100 0.781
2,150 0.789
λ [nm]
2,200 0.776
2,250 0.769
2,300 0.770
2,350 0.785
2,400 0.790
2,450 0.786
2,500 0.760
2,550 0.726
2,600 0.680
2,650 0.648
2,700 0.596
2,750 0.425
2,800 0.070
2,850 0.011
2,900 0.004
2,950 0.002
3,000 0.001
3,050 0.001
3,100 < 10⁻³
3,150 < 10⁻³
3,200 < 10⁻³
3,250 < 10⁻³
3,300 < 10⁻³
3,350 < 10⁻³
3,400 < 10⁻³
3,450 < 10⁻³
3,500 < 10⁻³
3,550 < 10⁻³
3,600 < 10⁻³
3,650 < 10⁻³
λ [nm]
3,700 0.001
3,750 0.001
3,800 0.001
3,850 0.001
3,900 < 10⁻³
3,950 < 10⁻³
4,000 < 10⁻³
4,050 < 10⁻³
4,100 < 10⁻³
4,150 < 10⁻³
4,200 < 10⁻³
4,250 < 10⁻³
4,300 < 10⁻³
4,350 < 10⁻³
4,400 < 10⁻³
4,450 < 10⁻³
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.915
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (350nm) ≥ 0,3
τi (405nm) ≥ 0,65
τi (514nm) ≥ 0,88
τi (633nm) ≤ 0,25
τi (694nm) ≤ 0,03
τi (1060nm) ≤ 0,0005
Refractive Indices n
nF (486.1 nm) = 1.539
nh (404.7 nm) = 1.546
ng (435.8 nm) = 1.543
ns (852.1 nm) = 1.528
ne (546.1 nm) = 1.536
nd (587.6 nm) = 1.534
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.361 0.309 0.275
y 0.441 0.459 0.472
Y 61 46 37
λd [nm] 502 501 501
Pe 0.20 0.31 0.39
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.340 0.292 0.260
y 0.426 0.441 0.451
Y 62 48 38
λd [nm] 500 500 500
Pe 0.20 0.32 0.39
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.255 0.225 0.206
y 0.335 0.340 0.346
Y 68 54 45
λd [nm] 493 493 493
Pe 0.21 0.31 0.38
Physical values
Density
p [g/cm3] 2.6751
Bubble content
Bubble class 2
Transformation temperature
Tg [°C] 457
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 2.0
AR class 2.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.44
α20°C/300°C [10-6/K] 8.88
α20°C/200°C [10-6/K]