BG36
Spectral values guaranteed
τi (405nm) ≥0.9
τi (450nm) ≤0.42
τi (800nm) ≤0.01
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
BG36 - BG36
Thickness
1.0
Reflection factor
0.8765
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 0.017
270 0.042
280 0.058
290 0.068
300 0.084
310 0.145
320 0.222
330 0.178
340 0.360
350 0.030
360 0.061
370 0.808
380 0.856
390 0.908
400 0.929
410 0.950
420 0.911
430 0.503
440 0.272
450 0.296
460 0.356
470 0.257
480 0.351
490 0.706
λ [nm]
500 0.608
510 0.168
520 0.162
530 0.139
540 0.708
550 0.905
560 0.837
570 0.019
580 < 10⁻³
590 0.002
600 0.241
610 0.851
620 0.904
630 0.890
640 0.965
650 0.996
660 0.984
670 0.816
680 0.579
690 0.771
700 0.929
710 0.953
720 0.850
730 0.153
740 0.003
750 0.005
760 0.146
770 0.578
780 0.459
790 0.042
λ [nm]
800 < 10⁻³
810 0.012
820 0.211
830 0.584
840 0.840
850 0.809
860 0.333
870 0.248
880 0.163
890 0.426
900 0.639
910 0.802
920 0.910
930 0.972
940 0.987
950 0.986
960 0.979
970 0.969
980 0.958
990 0.950
1,000 0.945
1,010 0.943
1,020 0.948
1,030 0.961
1,040 0.973
1,050 0.980
1,060 0.984
1,070 0.987
1,080 0.989
1,090 0.992
λ [nm]
1,100 0.995
1,110 0.996
1,120 0.996
1,130 0.997
1,140 0.998
1,150 0.998
1,160 0.998
1,170 0.997
1,180 0.997
1,190 0.996
1,200 0.995
1,250 0.995
1,300 0.989
1,350 0.869
1,400 0.513
1,450 0.411
1,500 0.193
1,550 0.236
1,600 0.475
1,650 0.689
1,700 0.824
1,750 0.873
1,800 0.795
1,850 0.595
1,900 0.443
1,950 0.471
2,000 0.574
2,050 0.660
2,100 0.723
2,150 0.768
λ [nm]
2,200 0.784
2,250 0.737
2,300 0.557
2,350 0.364
2,400 0.294
2,450 0.291
2,500 0.325
2,550 0.362
2,600 0.532
2,650 0.611
2,700 0.674
2,750 0.617
2,800 0.486
2,850 0.436
2,900 0.446
2,950 0.457
3,000 0.469
3,050 0.475
3,100 0.477
3,150 0.472
3,200 0.455
3,250 0.398
3,300 0.314
3,350 0.215
3,400 0.119
3,450 0.049
3,500 0.020
3,550 0.006
3,600 0.003
3,650 0.001
λ [nm]
3,700 < 10⁻³
3,750 < 10⁻³
3,800 < 10⁻³
3,850 < 10⁻³
3,900 < 10⁻³
3,950 0.001
4,000 < 10⁻³
4,050 < 10⁻³
4,100 < 10⁻³
4,150 < 10⁻³
4,200 < 10⁻³
4,250 < 10⁻³
4,300 < 10⁻³
4,350 < 10⁻³
4,400 < 10⁻³
4,450 < 10⁻³
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.877
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (405nm) ≥0.9
τi (450nm) ≤0.42
τi (800nm) ≤0.01
Refractive Indices n
nd (587.6 nm) = 1.690
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.495 0.534 0.557
y 0.387 0.390 0.389
Y 41 32 27
λd [nm] 628 600 599
Pe 0.19 0.48 0.63
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.469 0.512 0.537
y 0.382 0.390 0.391
Y 41 31 26
λd [nm] 629 599 597
Pe 0.16 0.44 0.59
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.344 0.395 0.429
y 0.327 0.356 0.370
Y 39 29 23
λd [nm] 622 591 590
Pe 0.08 0.30 0.44
Physical values
Density
p [g/cm3] 3.59
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 657
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 1
SR class 52.2
AR class 1.2
Thermal expansion
α-30°C/+70°C [10-6/K] 6.1
α20°C/300°C [10-6/K] 7.2
α20°C/200°C [10-6/K]