BG55

A NIR cutoff filter with a high steepness of NIR cutoff.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

BG55
Spectral values guaranteed
τi (405nm) ≥0.76
τi (514nm) ≥0.93
τi (633nm) ≥0.18
τi (694nm) ≤0.016
τi (1060nm) ≤0.0005
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
BG55 - BG55
Thickness
1.0
Reflection factor
0.9136
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300 < 10⁻³
310 0.007
320 0.092
330 0.265
340 0.421
350 0.528
360 0.598
370 0.650
380 0.693
390 0.731
400 0.765
410 0.794
420 0.821
430 0.845
440 0.866
450 0.884
460 0.900
470 0.913
480 0.925
490 0.934
λ [nm]
500 0.940
510 0.942
520 0.940
530 0.930
540 0.911
550 0.879
560 0.833
570 0.770
580 0.693
590 0.603
600 0.506
610 0.408
620 0.317
630 0.235
640 0.168
650 0.115
660 0.072
670 0.045
680 0.027
690 0.016
700 0.009
710 0.005
720 0.003
730 0.002
740 < 10⁻³
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 < 10⁻³
840 < 10⁻³
850 < 10⁻³
860 < 10⁻³
870 < 10⁻³
880 < 10⁻³
890 < 10⁻³
900 < 10⁻³
910 < 10⁻³
920 < 10⁻³
930 < 10⁻³
940 < 10⁻³
950 < 10⁻³
960 < 10⁻³
970 < 10⁻³
980 < 10⁻³
990 < 10⁻³
1,000 < 10⁻³
1,010 < 10⁻³
1,020 < 10⁻³
1,030 < 10⁻³
1,040 < 10⁻³
1,050 < 10⁻³
1,060 < 10⁻³
1,070 < 10⁻³
1,080 < 10⁻³
1,090 < 10⁻³
λ [nm]
1,100 < 10⁻³
1,110 < 10⁻³
1,120 < 10⁻³
1,130 < 10⁻³
1,140 0.001
1,150 0.001
1,160 0.002
1,170 0.002
1,180 0.003
1,190 0.003
1,200 0.004
1,250 0.009
1,300 0.021
1,350 0.040
1,400 0.072
1,450 0.115
1,500 0.171
1,550 0.237
1,600 0.309
1,650 0.384
1,700 0.456
1,750 0.524
1,800 0.584
1,850 0.638
1,900 0.684
1,950 0.724
2,000 0.754
2,050 0.781
2,100 0.803
2,150 0.813
λ [nm]
2,200 0.804
2,250 0.803
2,300 0.812
2,350 0.823
2,400 0.831
2,450 0.827
2,500 0.812
2,550 0.782
2,600 0.753
2,650 0.732
2,700 0.699
2,750 0.588
2,800 0.189
2,850 0.056
2,900 0.026
2,950 0.016
3,000 0.011
3,050 0.008
3,100 0.007
3,150 0.005
3,200 0.005
3,250 0.004
3,300 0.004
3,350 0.004
3,400 0.004
3,450 0.005
3,500 0.006
3,550 0.007
3,600 0.009
3,650 0.011
λ [nm]
3,700 0.012
3,750 0.011
3,800 0.010
3,850 0.008
3,900 0.006
3,950 0.004
4,000 0.003
4,050 0.002
4,100 0.001
4,150 < 10⁻³
4,200 < 10⁻³
4,250 < 10⁻³
4,300 0.001
4,350 0.002
4,400 0.003
4,450 0.004
4,500 0.006
4,550 0.007
4,600 0.008
4,650 0.010
4,700 0.012
4,750 0.014
4,800 0.016
4,850 0.018
4,900 0.019
4,950 0.019
5,000 0.016
5,050 0.012
5,100 0.008
5,150 0.004
Optical values
Reflection factor
Pd 0.914
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (405nm) ≥0.76
τi (514nm) ≥0.93
τi (633nm) ≥0.18
τi (694nm) ≤0.016
τi (1060nm) ≤0.0005
Refractive Indices n
nF (486.1 nm) = 1.546
nh (404.7 nm) = 1.554
ng (435.8 nm) = 1.550
ns (852.1 nm) = 1.532
ne (546.1 nm) = 1.542
nd (587.6 nm) = 1.540
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.356 0.302 0.267
y 0.438 0.452 0.460
Y 62 48 39
λd [nm] 501 500 500
Pe 0.21 0.33 0.41
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.336 0.285 0.252
y 0.423 0.432 0.437
Y 63 49 41
λd [nm] 499 498 498
Pe 0.21 0.34 0.42
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.252 0.220 0.201
y 0.329 0.328 0.328
Y 69 57 48
λd [nm] 492 491 491
Pe 0.22 0.34 0.41
Physical values
Density
p [g/cm3] 2.6522
Bubble content
Bubble class
Transformation temperature
Tg [°C] 453
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 2.0
AR class 2.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.22
α20°C/300°C [10-6/K] 9.05
α20°C/200°C [10-6/K]