BG62

A NIR cutoff filter with high humidity resistance.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

BG62
Spectral values guaranteed
τi (405nm) ≥0.73
τi (514nm) ≥0.89
τi (633nm) ≥0.08
τi (694nm) ≤0.005
τi (1060nm) ≤0.0005
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
BG62 - BG62
Thickness
1.0
Reflection factor
0.9150
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320 < 10⁻³
330 0.005
340 0.080
350 0.261
360 0.438
370 0.559
380 0.636
390 0.686
400 0.724
410 0.755
420 0.782
430 0.805
440 0.826
450 0.846
460 0.862
470 0.876
480 0.888
490 0.897
λ [nm]
500 0.901
510 0.900
520 0.890
530 0.870
540 0.836
550 0.786
560 0.718
570 0.633
580 0.536
590 0.435
600 0.335
610 0.245
620 0.169
630 0.112
640 0.069
650 0.041
660 0.023
670 0.013
680 0.007
690 0.003
700 0.002
710 < 10⁻³
720 < 10⁻³
730 < 10⁻³
740 < 10⁻³
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 < 10⁻³
840 < 10⁻³
850 < 10⁻³
860 < 10⁻³
870 < 10⁻³
880 < 10⁻³
890 < 10⁻³
900 < 10⁻³
910 < 10⁻³
920 < 10⁻³
930 < 10⁻³
940 < 10⁻³
950 < 10⁻³
960 < 10⁻³
970 < 10⁻³
980 < 10⁻³
990 < 10⁻³
1,000 < 10⁻³
1,010 < 10⁻³
1,020 < 10⁻³
1,030 < 10⁻³
1,040 < 10⁻³
1,050 < 10⁻³
1,060 < 10⁻³
1,070 < 10⁻³
1,080 < 10⁻³
1,090 < 10⁻³
λ [nm]
1,100 < 10⁻³
1,110 < 10⁻³
1,120 0.001
1,130 0.001
1,140 0.002
1,150 0.002
1,160 0.003
1,170 0.003
1,180 0.004
1,190 0.005
1,200 0.006
1,250 0.014
1,300 0.029
1,350 0.055
1,400 0.094
1,450 0.147
1,500 0.211
1,550 0.283
1,600 0.359
1,650 0.433
1,700 0.503
1,750 0.569
1,800 0.627
1,850 0.678
1,900 0.722
1,950 0.760
2,000 0.793
2,050 0.820
2,100 0.843
2,150 0.862
λ [nm]
2,200 0.876
2,250 0.886
2,300 0.896
2,350 0.905
2,400 0.913
2,450 0.918
2,500 0.919
2,550 0.921
2,600 0.921
2,650 0.921
2,700 0.918
2,750 0.907
2,800 0.858
2,850 0.770
2,900 0.689
2,950 0.627
3,000 0.575
3,050 0.529
3,100 0.485
3,150 0.443
3,200 0.406
3,250 0.375
3,300 0.349
3,350 0.328
3,400 0.313
3,450 0.304
3,500 0.300
3,550 0.303
3,600 0.312
3,650 0.326
λ [nm]
3,700 0.345
3,750 0.362
3,800 0.365
3,850 0.342
3,900 0.300
3,950 0.252
4,000 0.194
4,050 0.123
4,100 0.068
4,150 0.035
4,200 0.019
4,250 0.013
4,300 0.012
4,350 0.013
4,400 0.012
4,450 0.010
4,500 0.008
4,550 0.006
4,600 0.006
4,650 0.008
4,700 0.013
4,750 0.020
4,800 0.030
4,850 0.042
4,900 0.055
4,950 0.072
5,000 0.092
5,050 0.111
5,100 0.125
5,150 0.132
Optical values
Reflection factor
Pd 0.915
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (405nm) ≥0.73
τi (514nm) ≥0.89
τi (633nm) ≥0.08
τi (694nm) ≤0.005
τi (1060nm) ≤0.0005
Refractive Indices n
nF (486.1 nm) = 1.546
nh (404.7 nm) = 1.554
ng (435.8 nm) = 1.550
ns (852.1 nm) = 1.533
ne (546.1 nm) = 1.542
nd (587.6 nm) = 1.540
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.321 0.257 0.220
y 0.441 0.447 0.445
Y 52 36 27
λd [nm] 499 498 498
Pe 0.29 0.44 0.52
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.302 0.243 0.210
y 0.422 0.423 0.419
Y 53 38 29
λd [nm] 498 497 496
Pe 0.30 0.44 0.53
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.229 0.194 0.175
y 0.320 0.311 0.305
Y 60 45 36
λd [nm] 490 490 489
Pe 0.31 0.45 0.52
Physical values
Density
p [g/cm3] 2.848
Bubble content
Bubble class
Transformation temperature
Tg [°C] 410
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 1
SR class 52.3
AR class 3.3
Thermal expansion
α-30°C/+70°C [10-6/K] 11.92
α20°C/300°C [10-6/K] 13.62
α20°C/200°C [10-6/K]