A NIR cutoff filter with high humidity resistance.
Find more information in the tabs below or on our website.
Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.
For customized filter products you can mark an article and use the request-button.
*product image is exemplary.
Technical Details
Internal Transmittance (Chart)
- SCHOTT
- BG67 - BG67
- Thickness
- 1.0
- Reflection factor
- 0.9134
Internal Transmittance (Table)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | |
| 300 | |
| 310 | < 10⁻³ |
| 320 | < 10⁻³ |
| 330 | < 10⁻³ |
| 340 | 0.013 |
| 350 | 0.091 |
| 360 | 0.220 |
| 370 | 0.336 |
| 380 | 0.423 |
| 390 | 0.488 |
| 400 | 0.539 |
| 410 | 0.583 |
| 420 | 0.623 |
| 430 | 0.659 |
| 440 | 0.693 |
| 450 | 0.724 |
| 460 | 0.752 |
| 470 | 0.776 |
| 480 | 0.797 |
| 490 | 0.813 |
| λ [nm] | |
|---|---|
| 500 | 0.823 |
| 510 | 0.825 |
| 520 | 0.816 |
| 530 | 0.790 |
| 540 | 0.744 |
| 550 | 0.676 |
| 560 | 0.588 |
| 570 | 0.486 |
| 580 | 0.379 |
| 590 | 0.275 |
| 600 | 0.185 |
| 610 | 0.115 |
| 620 | 0.066 |
| 630 | 0.035 |
| 640 | 0.017 |
| 650 | 0.008 |
| 660 | 0.003 |
| 670 | 0.001 |
| 680 | < 10⁻³ |
| 690 | < 10⁻³ |
| 700 | < 10⁻³ |
| 710 | < 10⁻³ |
| 720 | < 10⁻³ |
| 730 | < 10⁻³ |
| 740 | < 10⁻³ |
| 750 | < 10⁻³ |
| 760 | < 10⁻³ |
| 770 | < 10⁻³ |
| 780 | < 10⁻³ |
| 790 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 800 | < 10⁻³ |
| 810 | < 10⁻³ |
| 820 | < 10⁻³ |
| 830 | < 10⁻³ |
| 840 | < 10⁻³ |
| 850 | < 10⁻³ |
| 860 | < 10⁻³ |
| 870 | < 10⁻³ |
| 880 | < 10⁻³ |
| 890 | < 10⁻³ |
| 900 | < 10⁻³ |
| 910 | < 10⁻³ |
| 920 | < 10⁻³ |
| 930 | < 10⁻³ |
| 940 | < 10⁻³ |
| 950 | < 10⁻³ |
| 960 | < 10⁻³ |
| 970 | < 10⁻³ |
| 980 | < 10⁻³ |
| 990 | < 10⁻³ |
| 1,000 | < 10⁻³ |
| 1,010 | < 10⁻³ |
| 1,020 | < 10⁻³ |
| 1,030 | < 10⁻³ |
| 1,040 | < 10⁻³ |
| 1,050 | < 10⁻³ |
| 1,060 | < 10⁻³ |
| 1,070 | < 10⁻³ |
| 1,080 | < 10⁻³ |
| 1,090 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 1,100 | < 10⁻³ |
| 1,110 | < 10⁻³ |
| 1,120 | < 10⁻³ |
| 1,130 | < 10⁻³ |
| 1,140 | < 10⁻³ |
| 1,150 | < 10⁻³ |
| 1,160 | < 10⁻³ |
| 1,170 | < 10⁻³ |
| 1,180 | < 10⁻³ |
| 1,190 | < 10⁻³ |
| 1,200 | < 10⁻³ |
| 1,250 | 0.002 |
| 1,300 | 0.005 |
| 1,350 | 0.013 |
| 1,400 | 0.026 |
| 1,450 | 0.053 |
| 1,500 | 0.092 |
| 1,550 | 0.145 |
| 1,600 | 0.207 |
| 1,650 | 0.277 |
| 1,700 | 0.349 |
| 1,750 | 0.421 |
| 1,800 | 0.490 |
| 1,850 | 0.552 |
| 1,900 | 0.608 |
| 1,950 | 0.658 |
| 2,000 | 0.701 |
| 2,050 | 0.738 |
| 2,100 | 0.770 |
| 2,150 | 0.796 |
| λ [nm] | |
|---|---|
| 2,200 | 0.816 |
| 2,250 | 0.834 |
| 2,300 | 0.849 |
| 2,350 | 0.862 |
| 2,400 | 0.872 |
| 2,450 | 0.880 |
| 2,500 | 0.884 |
| 2,550 | 0.887 |
| 2,600 | 0.887 |
| 2,650 | 0.886 |
| 2,700 | 0.881 |
| 2,750 | 0.865 |
| 2,800 | 0.797 |
| 2,850 | 0.682 |
| 2,900 | 0.582 |
| 2,950 | 0.507 |
| 3,000 | 0.448 |
| 3,050 | 0.396 |
| 3,100 | 0.350 |
| 3,150 | 0.308 |
| 3,200 | 0.272 |
| 3,250 | 0.243 |
| 3,300 | 0.219 |
| 3,350 | 0.202 |
| 3,400 | 0.190 |
| 3,450 | 0.183 |
| 3,500 | 0.180 |
| 3,550 | 0.183 |
| 3,600 | 0.191 |
| 3,650 | 0.204 |
| λ [nm] | |
|---|---|
| 3,700 | 0.222 |
| 3,750 | 0.239 |
| 3,800 | 0.246 |
| 3,850 | 0.232 |
| 3,900 | 0.204 |
| 3,950 | 0.170 |
| 4,000 | 0.127 |
| 4,050 | 0.077 |
| 4,100 | 0.041 |
| 4,150 | 0.021 |
| 4,200 | 0.011 |
| 4,250 | 0.008 |
| 4,300 | 0.007 |
| 4,350 | 0.008 |
| 4,400 | 0.007 |
| 4,450 | 0.006 |
| 4,500 | 0.005 |
| 4,550 | 0.004 |
| 4,600 | 0.004 |
| 4,650 | 0.006 |
| 4,700 | 0.009 |
| 4,750 | 0.015 |
| 4,800 | 0.022 |
| 4,850 | 0.031 |
| 4,900 | 0.041 |
| 4,950 | 0.055 |
| 5,000 | 0.071 |
| 5,050 | 0.086 |
| 5,100 | 0.098 |
| 5,150 | 0.102 |
Optical values
| Reflection factor | |
|---|---|
| Pd | 0.913 |
| Reference thickness | |
|---|---|
| d [mm] | 1 |
| Spectral values guaranteed | |
|---|---|
| τi (450nm) | ≥ 0,7 |
| τi (500nm) | ≥ 0,8 |
| τi (550nm) | ≥ 0,65 |
| τi (600nm) | ≤ 0,19 |
| Refractive Indices n |
|---|
| nF (486.1 nm) = 1.547 |
| nh (404.7 nm) = 1.556 |
| ng (435.8 nm) = 1.552 |
| ns (852.1 nm) = 1.533 |
| ne (546.1 nm) = 1.543 |
| nd (587.6 nm) = 1.541 |
Colorimetric evaluation
| Illuminant | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.285 | 0.222 | 0.189 |
| y | 0.450 | 0.456 | 0.457 |
| Y | 41 | 25 | 17 |
| λd [nm] | 499 | 498 | 498 |
| Pe | 0.37 | 0.52 | 0.59 |
| Illuminant | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.269 | 0.211 | 0.182 |
| y | 0.429 | 0.431 | 0.431 |
| Y | 43 | 27 | 19 |
| λd [nm] | 498 | 497 | 497 |
| Pe | 0.38 | 0.52 | 0.60 |
| Illuminant | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.209 | 0.176 | 0.159 |
| y | 0.321 | 0.317 | 0.318 |
| Y | 50 | 33 | 24 |
| λd [nm] | 491 | 490 | 491 |
| Pe | 0.38 | 0.51 | 0.57 |
Physical values
| Density | |
|---|---|
| p [g/cm3] | 2.8547 |
| Bubble content | |
|---|---|
| Bubble class | |
| Transformation temperature | |
|---|---|
| Tg [°C] | 390 |
| Temperature coefficient | |
|---|---|
| Tk [nm/°C] | |
| Chemical Resistance | |
|---|---|
| FR class | 1.0 |
| SR class | 52.3 |
| AR class | 3.3 |
| Thermal expansion | |
|---|---|
| α-30°C/+70°C [10-6/K] | 11.76 |
| α20°C/300°C [10-6/K] | 13.65 |
| α20°C/200°C [10-6/K] | |