GG420

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

GG420
Spectral values guaranteed
λs (τi = 0.00001) [nm] 360 nm
λc (τi = 0.5) [nm] 420 nm ± 6 nm
λp1 (τi = 0.93) [nm] 530 nm
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
GG420 - GG420
Thickness
3.0
Reflection factor
0.9183
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320
330
340
350
360 < 10⁻³
370 < 10⁻³
380 < 10⁻³
390 < 10⁻³
400 < 10⁻³
410 0.026
420 0.518
430 0.802
440 0.859
450 0.883
460 0.900
470 0.914
480 0.927
490 0.939
λ [nm]
500 0.949
510 0.958
520 0.964
530 0.970
540 0.975
550 0.979
560 0.982
570 0.985
580 0.986
590 0.987
600 0.988
610 0.988
620 0.988
630 0.988
640 0.987
650 0.986
660 0.986
670 0.985
680 0.984
690 0.983
700 0.982
710 0.981
720 0.980
730 0.978
740 0.977
750 0.976
760 0.974
770 0.973
780 0.971
790 0.970
λ [nm]
800 0.968
810 0.967
820 0.965
830 0.964
840 0.963
850 0.963
860 0.963
870 0.962
880 0.962
890 0.961
900 0.960
910 0.959
920 0.958
930 0.958
940 0.957
950 0.956
960 0.956
970 0.956
980 0.955
990 0.955
1,000 0.954
1,010 0.954
1,020 0.953
1,030 0.953
1,040 0.953
1,050 0.953
1,060 0.953
1,070 0.952
1,080 0.952
1,090 0.953
λ [nm]
1,100 0.952
1,110 0.953
1,120 0.952
1,130 0.953
1,140 0.953
1,150 0.952
1,160 0.953
1,170 0.952
1,180 0.953
1,190 0.953
1,200 0.953
1,250 0.954
1,300 0.956
1,350 0.958
1,400 0.958
1,450 0.963
1,500 0.968
1,550 0.971
1,600 0.974
1,650 0.975
1,700 0.975
1,750 0.975
1,800 0.974
1,850 0.971
1,900 0.970
1,950 0.968
2,000 0.965
2,050 0.963
2,100 0.959
2,150 0.955
λ [nm]
2,200 0.943
2,250 0.939
2,300 0.942
2,350 0.942
2,400 0.936
2,450 0.927
2,500 0.919
2,550 0.914
2,600 0.909
2,650 0.897
2,700 0.852
2,750 0.396
2,800 0.262
2,850 0.265
2,900 0.277
2,950 0.286
3,000 0.288
3,050 0.284
3,100 0.272
3,150 0.255
3,200 0.240
3,250 0.224
3,300 0.205
3,350 0.186
3,400 0.176
3,450 0.164
3,500 0.158
3,550 0.155
3,600 0.153
3,650 0.154
λ [nm]
3,700 0.157
3,750 0.164
3,800 0.172
3,850 0.177
3,900 0.178
3,950 0.174
4,000 0.166
4,050 0.155
4,100 0.141
4,150 0.123
4,200 0.105
4,250 0.086
4,300 0.066
4,350 0.046
4,400 0.024
4,450 0.009
4,500 0.003
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850
4,900
4,950
5,000
5,050
5,100
5,150
Optical values
Reflection factor
Pd 0.918
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 360 nm
λc (τi = 0.5) [nm] 420 nm ± 6 nm
λp1 (τi = 0.93) [nm] 530 nm
Refractive Indices n
ns (852.1 nm) = 1.520
ne (546.1 nm) = 1.530
nd (587.6 nm) = 1.520
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.450 0.453 0.455
y 0.410 0.412 0.414
Y 91 90 90
λd [nm] 581 581 581
Pe 0.04 0.07 0.10
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.426 0.429 0.432
y 0.403 0.405 0.408
Y 91 90 90
λd [nm] 579 579 579
Pe 0.04 0.07 0.10
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.317 0.320 0.324
y 0.337 0.342 0.348
Y 91 90 89
λd [nm] 569 570 570
Pe 0.03 0.06 0.08
Physical values
Density
p [g/cm3] 2.55
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 535
Temperature coefficient
Tk [nm/°C] 0.07
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.8
α20°C/300°C [10-6/K] 9
α20°C/200°C [10-6/K]