GG435

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

GG435
Spectral values guaranteed
λs (τi = 0.00001) [nm] 370 nm
λc (τi = 0.5) [nm] 435 nm ± 6 nm
λp1 (τi = 0.92) [nm] 520 nm
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
GG435 - GG435
Thickness
3.0
Reflection factor
0.9183
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 < 10⁻³
370 < 10⁻³
380 < 10⁻³
390 < 10⁻³
400 < 10⁻³
410 < 10⁻³
420 0.006
430 0.240
440 0.664
450 0.842
460 0.899
470 0.923
480 0.939
490 0.951
λ [nm]
500 0.960
510 0.967
520 0.972
530 0.977
540 0.980
550 0.983
560 0.985
570 0.986
580 0.987
590 0.987
600 0.987
610 0.986
620 0.986
630 0.985
640 0.984
650 0.983
660 0.982
670 0.981
680 0.980
690 0.978
700 0.977
710 0.976
720 0.974
730 0.973
740 0.971
750 0.969
760 0.967
770 0.965
780 0.963
790 0.962
λ [nm]
800 0.960
810 0.958
820 0.957
830 0.955
840 0.954
850 0.952
860 0.951
870 0.950
880 0.949
890 0.948
900 0.947
910 0.946
920 0.946
930 0.945
940 0.944
950 0.944
960 0.943
970 0.943
980 0.942
990 0.942
1,000 0.941
1,010 0.941
1,020 0.940
1,030 0.940
1,040 0.940
1,050 0.940
1,060 0.940
1,070 0.939
1,080 0.939
1,090 0.939
λ [nm]
1,100 0.939
1,110 0.939
1,120 0.939
1,130 0.939
1,140 0.939
1,150 0.939
1,160 0.939
1,170 0.940
1,180 0.940
1,190 0.940
1,200 0.940
1,250 0.941
1,300 0.943
1,350 0.946
1,400 0.947
1,450 0.953
1,500 0.958
1,550 0.962
1,600 0.965
1,650 0.967
1,700 0.967
1,750 0.967
1,800 0.965
1,850 0.963
1,900 0.962
1,950 0.960
2,000 0.958
2,050 0.956
2,100 0.954
2,150 0.948
λ [nm]
2,200 0.938
2,250 0.932
2,300 0.936
2,350 0.936
2,400 0.931
2,450 0.921
2,500 0.915
2,550 0.911
2,600 0.908
2,650 0.893
2,700 0.815
2,750 0.341
2,800 0.249
2,850 0.258
2,900 0.274
2,950 0.285
3,000 0.289
3,050 0.284
3,100 0.271
3,150 0.257
3,200 0.241
3,250 0.224
3,300 0.207
3,350 0.192
3,400 0.178
3,450 0.167
3,500 0.161
3,550 0.157
3,600 0.156
3,650 0.157
λ [nm]
3,700 0.161
3,750 0.169
3,800 0.176
3,850 0.180
3,900 0.182
3,950 0.177
4,000 0.168
4,050 0.156
4,100 0.140
4,150 0.122
4,200 0.103
4,250 0.082
4,300 0.059
4,350 0.039
4,400 0.021
4,450 0.009
4,500 0.003
4,550 0.001
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.918
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 370 nm
λc (τi = 0.5) [nm] 435 nm ± 6 nm
λp1 (τi = 0.92) [nm] 520 nm
Refractive Indices n
ns (852.1 nm) = 1.520
ne (546.1 nm) = 1.520
nd (587.6 nm) = 1.520
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.453 0.457 0.459
y 0.415 0.419 0.422
Y 91 91 90
λd [nm] 580 580 580
Pe 0.09 0.14 0.18
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.430 0.434 0.437
y 0.409 0.414 0.418
Y 91 90 90
λd [nm] 578 578 578
Pe 0.10 0.15 0.19
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.323 0.328 0.333
y 0.350 0.361 0.369
Y 91 90 90
λd [nm] 568 568 568
Pe 0.09 0.13 0.17
Physical values
Density
p [g/cm3] 2.55
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 537
Temperature coefficient
Tk [nm/°C] 0.08
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.8
α20°C/300°C [10-6/K] 9.1
α20°C/200°C [10-6/K]