OG530

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

OG530
Spectral values guaranteed
λs (τi = 0.00001) [nm] 460
λc (τi = 0.5) [nm] 530 ± 6
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
OG530 - OG530
Thickness
3.0
Reflection factor
0.9207
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 < 10⁻³
370 < 10⁻³
380 < 10⁻³
390 < 10⁻³
400 < 10⁻³
410 < 10⁻³
420 < 10⁻³
430 < 10⁻³
440 < 10⁻³
450 < 10⁻³
460 < 10⁻³
470 < 10⁻³
480 < 10⁻³
490 < 10⁻³
λ [nm]
500 < 10⁻³
510 0.005
520 0.136
530 0.514
540 0.802
550 0.919
560 0.961
570 0.976
580 0.982
590 0.985
600 0.986
610 0.986
620 0.986
630 0.986
640 0.985
650 0.985
660 0.984
670 0.983
680 0.982
690 0.981
700 0.980
710 0.978
720 0.977
730 0.976
740 0.974
750 0.973
760 0.971
770 0.970
780 0.968
790 0.966
λ [nm]
800 0.965
810 0.963
820 0.962
830 0.960
840 0.959
850 0.958
860 0.957
870 0.956
880 0.955
890 0.955
900 0.954
910 0.954
920 0.953
930 0.952
940 0.952
950 0.951
960 0.951
970 0.950
980 0.950
990 0.949
1,000 0.949
1,010 0.948
1,020 0.948
1,030 0.948
1,040 0.948
1,050 0.948
1,060 0.947
1,070 0.947
1,080 0.947
1,090 0.947
λ [nm]
1,100 0.947
1,110 0.947
1,120 0.947
1,130 0.948
1,140 0.948
1,150 0.948
1,160 0.948
1,170 0.948
1,180 0.948
1,190 0.948
1,200 0.948
1,250 0.950
1,300 0.951
1,350 0.954
1,400 0.955
1,450 0.959
1,500 0.964
1,550 0.967
1,600 0.970
1,650 0.972
1,700 0.972
1,750 0.972
1,800 0.970
1,850 0.968
1,900 0.966
1,950 0.963
2,000 0.961
2,050 0.958
2,100 0.956
2,150 0.952
λ [nm]
2,200 0.939
2,250 0.933
2,300 0.936
2,350 0.936
2,400 0.931
2,450 0.924
2,500 0.914
2,550 0.911
2,600 0.909
2,650 0.900
2,700 0.838
2,750 0.470
2,800 0.361
2,850 0.356
2,900 0.364
2,950 0.364
3,000 0.354
3,050 0.333
3,100 0.308
3,150 0.282
3,200 0.256
3,250 0.231
3,300 0.209
3,350 0.190
3,400 0.174
3,450 0.164
3,500 0.158
3,550 0.156
3,600 0.155
3,650 0.157
λ [nm]
3,700 0.162
3,750 0.168
3,800 0.175
3,850 0.182
3,900 0.189
3,950 0.193
4,000 0.188
4,050 0.176
4,100 0.158
4,150 0.134
4,200 0.110
4,250 0.085
4,300 0.063
4,350 0.043
4,400 0.023
4,450 0.010
4,500 0.004
4,550 0.002
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.921
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 460
λc (τi = 0.5) [nm] 530 ± 6
Refractive Indices n
ns (852.1 nm) = 1.510
ne (546.1 nm) = 1.510
nd (587.6 nm) = 1.510
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.534 0.545 0.550
y 0.457 0.452 0.447
Y 81 78 75
λd [nm] 584 585 586
Pe 0.94 0.98 0.98
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.524 0.536 0.542
y 0.466 0.460 0.454
Y 80 76 74
λd [nm] 583 584 585
Pe 0.94 0.98 0.99
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.476 0.496 0.505
y 0.501 0.498 0.490
Y 74 69 66
λd [nm] 576 578 579
Pe 0.94 0.99 0.99
Physical values
Density
p [g/cm3] 2.56
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 506
Temperature coefficient
Tk [nm/°C] 0.11
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.9
α20°C/300°C [10-6/K] 9
α20°C/200°C [10-6/K]