OG550

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

OG550
Spectral values guaranteed
λs (τi = 0.00001) [nm] 480
λc (τi = 0.5) [nm] 550 ± 6
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
OG550 - OG550
Thickness
3.0
Reflection factor
0.9201
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 < 10⁻³
370 < 10⁻³
380 < 10⁻³
390 < 10⁻³
400 < 10⁻³
410 < 10⁻³
420 < 10⁻³
430 < 10⁻³
440 < 10⁻³
450 < 10⁻³
460 < 10⁻³
470 < 10⁻³
480 < 10⁻³
490 < 10⁻³
λ [nm]
500 < 10⁻³
510 < 10⁻³
520 < 10⁻³
530 0.003
540 0.119
550 0.508
560 0.806
570 0.922
580 0.961
590 0.975
600 0.980
610 0.983
620 0.984
630 0.984
640 0.983
650 0.983
660 0.982
670 0.981
680 0.980
690 0.980
700 0.979
710 0.978
720 0.977
730 0.975
740 0.974
750 0.973
760 0.971
770 0.970
780 0.968
790 0.967
λ [nm]
800 0.965
810 0.963
820 0.962
830 0.961
840 0.960
850 0.959
860 0.958
870 0.957
880 0.957
890 0.956
900 0.955
910 0.955
920 0.954
930 0.953
940 0.953
950 0.952
960 0.952
970 0.951
980 0.951
990 0.950
1,000 0.950
1,010 0.950
1,020 0.949
1,030 0.949
1,040 0.949
1,050 0.949
1,060 0.949
1,070 0.949
1,080 0.949
1,090 0.949
λ [nm]
1,100 0.949
1,110 0.949
1,120 0.949
1,130 0.949
1,140 0.949
1,150 0.949
1,160 0.949
1,170 0.949
1,180 0.949
1,190 0.949
1,200 0.950
1,250 0.951
1,300 0.953
1,350 0.955
1,400 0.955
1,450 0.960
1,500 0.964
1,550 0.968
1,600 0.970
1,650 0.972
1,700 0.973
1,750 0.972
1,800 0.970
1,850 0.968
1,900 0.965
1,950 0.963
2,000 0.961
2,050 0.959
2,100 0.956
2,150 0.952
λ [nm]
2,200 0.938
2,250 0.933
2,300 0.936
2,350 0.935
2,400 0.932
2,450 0.925
2,500 0.919
2,550 0.911
2,600 0.901
2,650 0.886
2,700 0.833
2,750 0.456
2,800 0.354
2,850 0.351
2,900 0.363
2,950 0.368
3,000 0.357
3,050 0.336
3,100 0.306
3,150 0.273
3,200 0.246
3,250 0.224
3,300 0.205
3,350 0.188
3,400 0.175
3,450 0.166
3,500 0.160
3,550 0.155
3,600 0.153
3,650 0.156
λ [nm]
3,700 0.160
3,750 0.165
3,800 0.173
3,850 0.181
3,900 0.188
3,950 0.190
4,000 0.184
4,050 0.171
4,100 0.151
4,150 0.131
4,200 0.110
4,250 0.088
4,300 0.062
4,350 0.039
4,400 0.023
4,450 0.011
4,500 0.005
4,550 0.002
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.920
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 480
λc (τi = 0.5) [nm] 550 ± 6
Refractive Indices n
nF (486.1 nm) = 1.519
nh (404.7 nm) = 1.524
ng (435.8 nm) = 1.575
ns (852.1 nm) = 1.505
ne (546.1 nm) = 1.515
nd (587.6 nm) = 1.512
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.565 0.580 0.587
y 0.429 0.419 0.412
Y 70 65 62
λd [nm] 589 591 592
Pe 0.96 1.00 1.00
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.558 0.574 0.581
y 0.435 0.425 0.418
Y 68 63 59
λd [nm] 588 590 591
Pe 0.96 1.00 1.00
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.521 0.547 0.557
y 0.459 0.451 0.441
Y 58 52 49
λd [nm] 583 586 587
Pe 0.95 1.00 1.00
Physical values
Density
p [g/cm3] 2.56
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 507
Temperature coefficient
Tk [nm/°C] 0.12
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.9
α20°C/300°C [10-6/K] 9
α20°C/200°C [10-6/K]