OG570

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

OG570
Spectral values guaranteed
λs (τi = 0.00001) [nm] 500 nm
λc (τi = 0.5) [nm] 570 nm ± 6 nm
λp1 (τi = 0.93) [nm] 640 nm
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
OG570 - OG570
Thickness
3.0
Reflection factor
0.9207
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320
330
340
350
360
370
380
390
400
410
420
430
440
450
460
470
480 < 10⁻³
490 < 10⁻³
λ [nm]
500 < 10⁻³
510 < 10⁻³
520 < 10⁻³
530 < 10⁻³
540 < 10⁻³
550 < 10⁻³
560 0.029
570 0.330
580 0.739
590 0.913
600 0.963
610 0.976
620 0.981
630 0.982
640 0.982
650 0.982
660 0.981
670 0.980
680 0.979
690 0.978
700 0.977
710 0.976
720 0.975
730 0.974
740 0.972
750 0.971
760 0.969
770 0.968
780 0.966
790 0.964
λ [nm]
800 0.963
810 0.961
820 0.960
830 0.959
840 0.957
850 0.956
860 0.955
870 0.954
880 0.953
890 0.953
900 0.952
910 0.951
920 0.951
930 0.950
940 0.950
950 0.949
960 0.949
970 0.948
980 0.948
990 0.948
1,000 0.947
1,010 0.947
1,020 0.946
1,030 0.946
1,040 0.946
1,050 0.946
1,060 0.946
1,070 0.946
1,080 0.946
1,090 0.946
λ [nm]
1,100 0.946
1,110 0.946
1,120 0.946
1,130 0.946
1,140 0.946
1,150 0.946
1,160 0.946
1,170 0.947
1,180 0.947
1,190 0.947
1,200 0.947
1,250 0.948
1,300 0.950
1,350 0.953
1,400 0.953
1,450 0.958
1,500 0.963
1,550 0.966
1,600 0.969
1,650 0.971
1,700 0.971
1,750 0.970
1,800 0.969
1,850 0.967
1,900 0.964
1,950 0.962
2,000 0.960
2,050 0.957
2,100 0.954
2,150 0.950
λ [nm]
2,200 0.936
2,250 0.933
2,300 0.935
2,350 0.934
2,400 0.930
2,450 0.922
2,500 0.912
2,550 0.911
2,600 0.912
2,650 0.899
2,700 0.829
2,750 0.455
2,800 0.354
2,850 0.357
2,900 0.367
2,950 0.368
3,000 0.353
3,050 0.332
3,100 0.305
3,150 0.276
3,200 0.251
3,250 0.229
3,300 0.209
3,350 0.191
3,400 0.173
3,450 0.160
3,500 0.154
3,550 0.154
3,600 0.157
3,650 0.162
λ [nm]
3,700 0.167
3,750 0.173
3,800 0.179
3,850 0.184
3,900 0.188
3,950 0.189
4,000 0.184
4,050 0.170
4,100 0.150
4,150 0.130
4,200 0.109
4,250 0.088
4,300 0.066
4,350 0.044
4,400 0.025
4,450 0.011
4,500 0.005
4,550 0.002
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.921
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 500 nm
λc (τi = 0.5) [nm] 570 nm ± 6 nm
λp1 (τi = 0.93) [nm] 640 nm
Refractive Indices n
ns (852.1 nm) = 1.510
nd (587.6 nm) = 1.510
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.600 0.619 0.627
y 0.394 0.380 0.372
Y 56 49 46
λd [nm] 596 598 600
Pe 0.96 1.00 1.00
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.595 0.616 0.624
y 0.398 0.384 0.375
Y 53 47 44
λd [nm] 595 598 599
Pe 0.96 1.00 1.00
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.566 0.600 0.611
y 0.412 0.399 0.389
Y 43 36 33
λd [nm] 591 595 597
Pe 0.94 1.00 1.00
Physical values
Density
p [g/cm3] 2.6137
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 510
Temperature coefficient
Tk [nm/°C] 0.12
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.9
α20°C/300°C [10-6/K] 9
α20°C/200°C [10-6/K]