Technical Details
Internal Transmittance (Chart)
- SCHOTT
- S8022 - S8022
- Thickness
- 2.0
- Reflection factor
- 0.9099
Internal Transmittance (Table)
| λ [nm] | |
|---|---|
| 200 | < 10⁻³ |
| 210 | < 10⁻³ |
| 220 | < 10⁻³ |
| 230 | < 10⁻³ |
| 240 | < 10⁻³ |
| 250 | < 10⁻³ |
| 260 | < 10⁻³ |
| 270 | < 10⁻³ |
| 280 | < 10⁻³ |
| 290 | < 10⁻³ |
| 300 | < 10⁻³ |
| 310 | < 10⁻³ |
| 320 | < 10⁻³ |
| 330 | < 10⁻³ |
| 340 | < 10⁻³ |
| 350 | < 10⁻³ |
| 360 | < 10⁻³ |
| 370 | 0.005 |
| 380 | 0.018 |
| 390 | 0.040 |
| 400 | 0.065 |
| 410 | 0.096 |
| 420 | 0.120 |
| 430 | 0.141 |
| 440 | 0.163 |
| 450 | 0.188 |
| 460 | 0.221 |
| 470 | 0.262 |
| 480 | 0.316 |
| 490 | 0.380 |
| λ [nm] | |
|---|---|
| 500 | 0.448 |
| 510 | 0.505 |
| 520 | 0.531 |
| 530 | 0.512 |
| 540 | 0.443 |
| 550 | 0.337 |
| 560 | 0.220 |
| 570 | 0.120 |
| 580 | 0.053 |
| 590 | 0.017 |
| 600 | 0.005 |
| 610 | < 10⁻³ |
| 620 | < 10⁻³ |
| 630 | < 10⁻³ |
| 640 | < 10⁻³ |
| 650 | < 10⁻³ |
| 660 | < 10⁻³ |
| 670 | < 10⁻³ |
| 680 | < 10⁻³ |
| 690 | < 10⁻³ |
| 700 | < 10⁻³ |
| 710 | < 10⁻³ |
| 720 | < 10⁻³ |
| 730 | < 10⁻³ |
| 740 | < 10⁻³ |
| 750 | < 10⁻³ |
| 760 | < 10⁻³ |
| 770 | < 10⁻³ |
| 780 | < 10⁻³ |
| 790 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 800 | < 10⁻³ |
| 810 | < 10⁻³ |
| 820 | < 10⁻³ |
| 830 | < 10⁻³ |
| 840 | < 10⁻³ |
| 850 | < 10⁻³ |
| 860 | < 10⁻³ |
| 870 | < 10⁻³ |
| 880 | < 10⁻³ |
| 890 | < 10⁻³ |
| 900 | < 10⁻³ |
| 910 | < 10⁻³ |
| 920 | < 10⁻³ |
| 930 | < 10⁻³ |
| 940 | < 10⁻³ |
| 950 | < 10⁻³ |
| 960 | < 10⁻³ |
| 970 | < 10⁻³ |
| 980 | < 10⁻³ |
| 990 | < 10⁻³ |
| 1,000 | < 10⁻³ |
| 1,010 | < 10⁻³ |
| 1,020 | < 10⁻³ |
| 1,030 | < 10⁻³ |
| 1,040 | < 10⁻³ |
| 1,050 | < 10⁻³ |
| 1,060 | < 10⁻³ |
| 1,070 | < 10⁻³ |
| 1,080 | < 10⁻³ |
| 1,090 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 1,100 | < 10⁻³ |
| 1,110 | < 10⁻³ |
| 1,120 | < 10⁻³ |
| 1,130 | < 10⁻³ |
| 1,140 | < 10⁻³ |
| 1,150 | < 10⁻³ |
| 1,160 | < 10⁻³ |
| 1,170 | < 10⁻³ |
| 1,180 | < 10⁻³ |
| 1,190 | < 10⁻³ |
| 1,200 | < 10⁻³ |
| 1,250 | < 10⁻³ |
| 1,300 | < 10⁻³ |
| 1,350 | < 10⁻³ |
| 1,400 | < 10⁻³ |
| 1,450 | < 10⁻³ |
| 1,500 | < 10⁻³ |
| 1,550 | < 10⁻³ |
| 1,600 | < 10⁻³ |
| 1,650 | 0.003 |
| 1,700 | 0.007 |
| 1,750 | 0.016 |
| 1,800 | 0.031 |
| 1,850 | 0.053 |
| 1,900 | 0.083 |
| 1,950 | 0.120 |
| 2,000 | 0.162 |
| 2,050 | 0.207 |
| 2,100 | 0.255 |
| 2,150 | 0.302 |
| λ [nm] | |
|---|---|
| 2,200 | 0.345 |
| 2,250 | 0.387 |
| 2,300 | 0.429 |
| 2,350 | 0.469 |
| 2,400 | 0.506 |
| 2,450 | 0.538 |
| 2,500 | 0.562 |
| 2,550 | 0.577 |
| 2,600 | 0.590 |
| 2,650 | 0.602 |
| 2,700 | 0.606 |
| 2,750 | 0.571 |
| 2,800 | 0.374 |
| 2,850 | 0.213 |
| 2,900 | 0.142 |
| 2,950 | 0.107 |
| 3,000 | 0.086 |
| 3,050 | 0.071 |
| 3,100 | 0.059 |
| 3,150 | 0.050 |
| 3,200 | 0.044 |
| 3,250 | 0.039 |
| 3,300 | 0.037 |
| 3,350 | 0.036 |
| 3,400 | 0.036 |
| 3,450 | 0.037 |
| 3,500 | 0.040 |
| 3,550 | 0.044 |
| 3,600 | 0.049 |
| 3,650 | 0.054 |
| λ [nm] | |
|---|---|
| 3,700 | 0.058 |
| 3,750 | 0.055 |
| 3,800 | 0.044 |
| 3,850 | 0.031 |
| 3,900 | 0.019 |
| 3,950 | 0.009 |
| 4,000 | 0.004 |
| 4,050 | 0.001 |
| 4,100 | < 10⁻³ |
| 4,150 | < 10⁻³ |
| 4,200 | < 10⁻³ |
| 4,250 | < 10⁻³ |
| 4,300 | < 10⁻³ |
| 4,350 | < 10⁻³ |
| 4,400 | < 10⁻³ |
| 4,450 | < 10⁻³ |
| 4,500 | < 10⁻³ |
| 4,550 | < 10⁻³ |
| 4,600 | < 10⁻³ |
| 4,650 | < 10⁻³ |
| 4,700 | < 10⁻³ |
| 4,750 | 0.001 |
| 4,800 | 0.002 |
| 4,850 | 0.003 |
| 4,900 | 0.003 |
| 4,950 | 0.003 |
| 5,000 | 0.003 |
| 5,050 | 0.002 |
| 5,100 | 0.001 |
| 5,150 | < 10⁻³ |
Optical values
| Reflection factor | |
|---|---|
| Pd | 0.910 |
| Reference thickness | |
|---|---|
| d [mm] | 2 |
| Refractive Indices n |
|---|
| nF (486.1 nm) = 1.564 |
| nh (404.7 nm) = 1.576 |
| ng (435.8 nm) = 1.570 |
| ns (852.1 nm) = 1.549 |
| ne (546.1 nm) = 1.560 |
| nd (587.6 nm) = |
Colorimetric evaluation
| Illuminant | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.253 | 0.203 | 0.178 |
| y | 0.498 | 0.549 | 0.593 |
| Y | 30 | 16 | 9 |
| λd [nm] | 503 | 505 | 508 |
| Pe | 0.44 | 0.55 | 0.61 |
| Illuminant | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.241 | 0.196 | 0.173 |
| y | 0.478 | 0.530 | 0.577 |
| Y | 31 | 16 | 10 |
| λd [nm] | 502 | 504 | 507 |
| Pe | 0.44 | 0.54 | 0.60 |
| Illuminant | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.196 | 0.169 | 0.154 |
| y | 0.374 | 0.432 | 0.492 |
| Y | 37 | 21 | 12 |
| λd [nm] | 496 | 500 | 505 |
| Pe | 0.40 | 0.47 | 0.51 |
Physical values
| Density | |
|---|---|
| p [g/cm3] | 2.77 |
| Bubble content | |
|---|---|
| Bubble class | |
| Transformation temperature | |
|---|---|
| Tg [°C] | 453 |
| Temperature coefficient | |
|---|---|
| Tk [nm/°C] | |
| Chemical Resistance | |
|---|---|
| FR class | |
| SR class | 4.0 |
| AR class | 3.0 |
| Thermal expansion | |
|---|---|
| α-30°C/+70°C [10-6/K] | 7.8 |
| α20°C/300°C [10-6/K] | 8.9 |
| α20°C/200°C [10-6/K] | |