S8023

Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
S8023 - S8023
Thickness
3.0
Reflection factor
0.9133
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 0.012
370 0.064
380 0.140
390 0.210
400 0.259
410 0.288
420 0.304
430 0.314
440 0.325
450 0.343
460 0.372
470 0.410
480 0.461
490 0.521
λ [nm]
500 0.580
510 0.619
520 0.622
530 0.575
540 0.480
550 0.353
560 0.222
570 0.116
580 0.049
590 0.016
600 0.004
610 < 10⁻³
620 < 10⁻³
630 < 10⁻³
640 < 10⁻³
650 < 10⁻³
660 < 10⁻³
670 < 10⁻³
680 < 10⁻³
690 < 10⁻³
700 < 10⁻³
710 < 10⁻³
720 < 10⁻³
730 < 10⁻³
740 < 10⁻³
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 < 10⁻³
840 < 10⁻³
850 < 10⁻³
860 < 10⁻³
870 < 10⁻³
880 < 10⁻³
890 < 10⁻³
900 < 10⁻³
910 < 10⁻³
920 < 10⁻³
930 < 10⁻³
940 < 10⁻³
950 < 10⁻³
960 < 10⁻³
970 < 10⁻³
980 < 10⁻³
990 < 10⁻³
1,000 < 10⁻³
1,010 < 10⁻³
1,020 < 10⁻³
1,030 < 10⁻³
1,040 < 10⁻³
1,050 < 10⁻³
1,060 < 10⁻³
1,070 < 10⁻³
1,080 < 10⁻³
1,090 < 10⁻³
λ [nm]
1,100 < 10⁻³
1,110 < 10⁻³
1,120 < 10⁻³
1,130 < 10⁻³
1,140 < 10⁻³
1,150 < 10⁻³
1,160 < 10⁻³
1,170 < 10⁻³
1,180 < 10⁻³
1,190 < 10⁻³
1,200 < 10⁻³
1,250 < 10⁻³
1,300 < 10⁻³
1,350 < 10⁻³
1,400 < 10⁻³
1,450 < 10⁻³
1,500 < 10⁻³
1,550 < 10⁻³
1,600 < 10⁻³
1,650 0.001
1,700 0.004
1,750 0.011
1,800 0.024
1,850 0.044
1,900 0.072
1,950 0.107
2,000 0.149
2,050 0.195
2,100 0.243
2,150 0.291
λ [nm]
2,200 0.332
2,250 0.373
2,300 0.414
2,350 0.453
2,400 0.489
2,450 0.519
2,500 0.537
2,550 0.545
2,600 0.550
2,650 0.555
2,700 0.548
2,750 0.499
2,800 0.269
2,850 0.112
2,900 0.059
2,950 0.037
3,000 0.026
3,050 0.018
3,100 0.013
3,150 0.010
3,200 0.007
3,250 0.006
3,300 0.005
3,350 0.004
3,400 0.004
3,450 0.004
3,500 0.005
3,550 0.005
3,600 0.006
3,650 0.008
λ [nm]
3,700 0.009
3,750 0.008
3,800 0.005
3,850 0.003
3,900 0.001
3,950 < 10⁻³
4,000 < 10⁻³
4,050 < 10⁻³
4,100 < 10⁻³
4,150 < 10⁻³
4,200 < 10⁻³
4,250 < 10⁻³
4,300 < 10⁻³
4,350 < 10⁻³
4,400 < 10⁻³
4,450 < 10⁻³
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.913
Reference thickness
d [mm] 3
Refractive Indices n
nF (486.1 nm) = 1.548
nh (404.7 nm) = 1.568
ng (435.8 nm) = 1.556
ns (852.1 nm) = 1.537
ne (546.1 nm) = 1.544
nd (587.6 nm) =
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.277 0.218 0.189
y 0.459 0.474 0.486
Y 41 27 19
λd [nm] 500 500 500
Pe 0.39 0.52 0.59
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.262 0.209 0.182
y 0.437 0.449 0.460
Y 43 28 21
λd [nm] 498 498 499
Pe 0.39 0.52 0.59
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.206 0.176 0.160
y 0.328 0.334 0.346
Y 51 35 26
λd [nm] 491 492 493
Pe 0.39 0.50 0.54
Physical values
Density
p [g/cm3] 2.75
Bubble content
Bubble class
Transformation temperature
Tg [°C] 444
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 4.0
AR class 3.0
Thermal expansion
α-30°C/+70°C [10-6/K]
α20°C/300°C [10-6/K]
α20°C/200°C [10-6/K] 9.7