Technical Details
Internal Transmittance (Chart)
- SCHOTT
- BG26 - BG26
- Thickness
- 1.0
- Reflection factor
- 0.9213
Internal Transmittance (Table)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | < 10⁻³ |
| 290 | 0.005 |
| 300 | 0.079 |
| 310 | 0.314 |
| 320 | 0.595 |
| 330 | 0.785 |
| 340 | 0.888 |
| 350 | 0.940 |
| 360 | 0.964 |
| 370 | 0.977 |
| 380 | 0.982 |
| 390 | 0.986 |
| 400 | 0.989 |
| 410 | 0.990 |
| 420 | 0.991 |
| 430 | 0.992 |
| 440 | 0.992 |
| 450 | 0.993 |
| 460 | 0.993 |
| 470 | 0.993 |
| 480 | 0.991 |
| 490 | 0.989 |
| λ [nm] | |
|---|---|
| 500 | 0.985 |
| 510 | 0.979 |
| 520 | 0.971 |
| 530 | 0.960 |
| 540 | 0.946 |
| 550 | 0.931 |
| 560 | 0.913 |
| 570 | 0.893 |
| 580 | 0.871 |
| 590 | 0.848 |
| 600 | 0.824 |
| 610 | 0.800 |
| 620 | 0.776 |
| 630 | 0.752 |
| 640 | 0.729 |
| 650 | 0.707 |
| 660 | 0.687 |
| 670 | 0.668 |
| 680 | 0.651 |
| 690 | 0.636 |
| 700 | 0.624 |
| 710 | 0.611 |
| 720 | 0.601 |
| 730 | 0.593 |
| 740 | 0.586 |
| 750 | 0.580 |
| 760 | 0.576 |
| 770 | 0.572 |
| 780 | 0.570 |
| 790 | 0.569 |
| λ [nm] | |
|---|---|
| 800 | 0.568 |
| 810 | 0.569 |
| 820 | 0.570 |
| 830 | 0.572 |
| 840 | 0.575 |
| 850 | 0.578 |
| 860 | 0.582 |
| 870 | 0.586 |
| 880 | 0.591 |
| 890 | 0.596 |
| 900 | 0.603 |
| 910 | 0.609 |
| 920 | 0.616 |
| 930 | 0.623 |
| 940 | 0.630 |
| 950 | 0.637 |
| 960 | 0.645 |
| 970 | 0.652 |
| 980 | 0.659 |
| 990 | 0.667 |
| 1,000 | 0.674 |
| 1,010 | 0.681 |
| 1,020 | 0.689 |
| 1,030 | 0.696 |
| 1,040 | 0.703 |
| 1,050 | 0.710 |
| 1,060 | 0.717 |
| 1,070 | 0.724 |
| 1,080 | 0.730 |
| 1,090 | 0.737 |
| λ [nm] | |
|---|---|
| 1,100 | 0.743 |
| 1,110 | 0.750 |
| 1,120 | 0.756 |
| 1,130 | 0.762 |
| 1,140 | 0.768 |
| 1,150 | 0.774 |
| 1,160 | 0.780 |
| 1,170 | 0.785 |
| 1,180 | 0.791 |
| 1,190 | 0.796 |
| 1,200 | 0.801 |
| 1,250 | 0.826 |
| 1,300 | 0.848 |
| 1,350 | 0.867 |
| 1,400 | 0.884 |
| 1,450 | 0.898 |
| 1,500 | 0.910 |
| 1,550 | 0.921 |
| 1,600 | 0.930 |
| 1,650 | 0.938 |
| 1,700 | 0.944 |
| 1,750 | 0.950 |
| 1,800 | 0.954 |
| 1,850 | 0.957 |
| 1,900 | 0.960 |
| 1,950 | 0.962 |
| 2,000 | 0.964 |
| 2,050 | 0.965 |
| 2,100 | 0.967 |
| 2,150 | 0.967 |
| λ [nm] | |
|---|---|
| 2,200 | 0.963 |
| 2,250 | 0.962 |
| 2,300 | 0.962 |
| 2,350 | 0.963 |
| 2,400 | 0.962 |
| 2,450 | 0.958 |
| 2,500 | 0.955 |
| 2,550 | < 10⁻³ |
| 2,600 | < 10⁻³ |
| 2,650 | < 10⁻³ |
| 2,700 | < 10⁻³ |
| 2,750 | < 10⁻³ |
| 2,800 | < 10⁻³ |
| 2,850 | < 10⁻³ |
| 2,900 | < 10⁻³ |
| 2,950 | < 10⁻³ |
| 3,000 | < 10⁻³ |
| 3,050 | < 10⁻³ |
| 3,100 | < 10⁻³ |
| 3,150 | < 10⁻³ |
| 3,200 | < 10⁻³ |
| 3,250 | < 10⁻³ |
| 3,300 | < 10⁻³ |
| 3,350 | < 10⁻³ |
| 3,400 | < 10⁻³ |
| 3,450 | < 10⁻³ |
| 3,500 | < 10⁻³ |
| 3,550 | < 10⁻³ |
| 3,600 | < 10⁻³ |
| 3,650 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 3,700 | < 10⁻³ |
| 3,750 | < 10⁻³ |
| 3,800 | < 10⁻³ |
| 3,850 | < 10⁻³ |
| 3,900 | < 10⁻³ |
| 3,950 | < 10⁻³ |
| 4,000 | < 10⁻³ |
| 4,050 | < 10⁻³ |
| 4,100 | < 10⁻³ |
| 4,150 | < 10⁻³ |
| 4,200 | < 10⁻³ |
| 4,250 | < 10⁻³ |
| 4,300 | < 10⁻³ |
| 4,350 | < 10⁻³ |
| 4,400 | < 10⁻³ |
| 4,450 | < 10⁻³ |
| 4,500 | < 10⁻³ |
| 4,550 | < 10⁻³ |
| 4,600 | < 10⁻³ |
| 4,650 | < 10⁻³ |
| 4,700 | < 10⁻³ |
| 4,750 | < 10⁻³ |
| 4,800 | < 10⁻³ |
| 4,850 | < 10⁻³ |
| 4,900 | < 10⁻³ |
| 4,950 | < 10⁻³ |
| 5,000 | < 10⁻³ |
| 5,050 | < 10⁻³ |
| 5,100 | < 10⁻³ |
| 5,150 | < 10⁻³ |
Optical values
| Reflection factor | |
|---|---|
| Pd | 0.921 |
| Reference thickness | |
|---|---|
| d [mm] | 1 |
| Spectral values guaranteed | |
|---|---|
| τi (450nm) | ≥ 0,98 |
| τi (633nm) | ≤ 0,79 |
| τi (800nm) | ≤ 0,62 |
| Refractive Indices n |
|---|
| nF (486.1 nm) = 1.516 |
| nh (404.7 nm) = 1.525 |
| ng (435.8 nm) = 1.521 |
| ns (852.1 nm) = 1.502 |
| ne (546.1 nm) = 1.512 |
| nd (587.6 nm) = 1.510 |
Colorimetric evaluation
| Illuminant | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| Illuminant | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
| Illuminant | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | |||
| y | |||
| Y | |||
| λd [nm] | |||
| Pe | |||
Physical values
| Density | |
|---|---|
| p [g/cm3] | |
| Bubble content | |
|---|---|
| Bubble class | |
| Transformation temperature | |
|---|---|
| Tg [°C] | 478 |
| Temperature coefficient | |
|---|---|
| Tk [nm/°C] | |
| Chemical Resistance | |
|---|---|
| FR class | - |
| SR class | - |
| AR class | - |
| Thermal expansion | |
|---|---|
| α-30°C/+70°C [10-6/K] | |
| α20°C/300°C [10-6/K] | |
| α20°C/200°C [10-6/K] | |