N-WG360

N-WG360
Spectral values guaranteed
λs (τi = 0.00001) [nm] 335
λc (τi = 0.5) [nm] 360 ± 6
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
N-WG360 - N-WG360
Thickness
2.0
Reflection factor
0.9175
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320
330
340 < 10⁻³
350 0.069
360 0.500
370 0.831
380 0.933
390 0.964
400 0.974
410 0.979
420 0.983
430 0.984
440 0.985
450 0.986
460 0.987
470 0.988
480 0.989
490 0.990
λ [nm]
500 0.991
510 0.990
520 0.990
530 0.991
540 0.991
550 0.991
560 0.991
570 0.992
580 0.992
590 0.992
600 0.993
610 0.992
620 0.993
630 0.993
640 0.993
650 0.993
660 0.994
670 0.994
680 0.994
690 0.995
700 0.994
710 0.995
720 0.996
730 0.995
740 0.996
750 0.994
760 0.996
770 0.996
780 0.995
790 0.995
λ [nm]
800 0.996
810 0.995
820 0.995
830 0.992
840 0.998
850 0.998
860 0.995
870 0.996
880 0.994
890 0.995
900 0.996
910 0.997
920 0.996
930 0.997
940 0.996
950 0.996
960 0.996
970 0.996
980 0.996
990 0.995
1,000 0.997
1,010 0.997
1,020 0.997
1,030 0.997
1,040 0.998
1,050 0.997
1,060 0.997
1,070 0.996
1,080 0.997
1,090 0.997
λ [nm]
1,100 0.997
1,110 0.997
1,120 0.996
1,130 0.997
1,140 0.997
1,150 0.998
1,160 0.997
1,170 0.997
1,180 0.998
1,190 0.998
1,200 0.997
1,250 0.998
1,300 0.998
1,350 0.997
1,400 0.994
1,450 0.995
1,500 0.997
1,550 0.997
1,600 0.995
1,650 0.995
1,700 0.994
1,750 0.990
1,800 0.987
1,850 0.984
1,900 0.980
1,950 0.977
2,000 0.972
2,050 0.968
2,100 0.958
2,150 0.954
λ [nm]
2,200 0.936
2,250 0.928
2,300 0.931
2,350 0.928
2,400 0.918
2,450 0.910
2,500 0.896
2,550 0.887
2,600 0.876
2,650 0.858
2,700 0.795
2,750 0.360
2,800 0.238
2,850 0.241
2,900 0.255
2,950 0.266
3,000 0.268
3,050 0.259
3,100 0.242
3,150 0.220
3,200 0.196
3,250 0.173
3,300 0.151
3,350 0.132
3,400 0.116
3,450 0.104
3,500 0.095
3,550 0.090
3,600 0.089
3,650 0.090
λ [nm]
3,700 0.092
3,750 0.096
3,800 0.102
3,850 0.109
3,900 0.116
3,950 0.120
4,000 0.120
4,050 0.113
4,100 0.100
4,150 0.084
4,200 0.069
4,250 0.056
4,300 0.044
4,350 0.034
4,400 0.024
4,450 0.015
4,500 0.008
4,550 0.004
4,600 0.001
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.918
Reference thickness
d [mm] 2
Spectral values guaranteed
λs (τi = 0.00001) [nm] 335
λc (τi = 0.5) [nm] 360 ± 6
Refractive Indices n
nF (486.1 nm) = 1.532
nh (404.7 nm) = 1.540
ng (435.8 nm) = 1.536
ns (852.1 nm) = 1.518
ne (546.1 nm) = 1.528
nd (587.6 nm) = 1.526
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.448 0.448 0.448
y 0.408 0.408 0.408
Y 91 91 91
λd [nm] 585 585 585
Pe 0.00 0.00 0.01
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.424 0.424 0.424
y 0.399 0.399 0.399
Y 91 91 91
λd [nm] 583 583 583
Pe 0.00 0.00 0.01
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.313 0.313 0.313
y 0.329 0.330 0.330
Y 91 91 91
λd [nm] 575 575 575
Pe 0.00 0.00 0.00
Physical values
Density
p [g/cm3] 2.6919
Bubble content
Bubble class -
Transformation temperature
Tg [°C] 522
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 1.0
AR class 2.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.83
α20°C/300°C [10-6/K] 8.85
α20°C/200°C [10-6/K]