RG905

A longpass filter with low transmission in short wavelengths range and high transmission in long wavelength ranges. They seperate visible from infrared light.

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

RG905.jpeg
Spectral values guaranteed
τi (405nm) ≤ 0,002
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
RG905 - RG905
Thickness
4.0
Reflection factor
0.9210
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340
350
360
370
380
390 < 10⁻³
400 < 10⁻³
410 < 10⁻³
420 < 10⁻³
430 < 10⁻³
440 < 10⁻³
450 0.003
460 0.011
470 0.027
480 0.041
490 0.045
λ [nm]
500 0.041
510 0.027
520 0.014
530 0.005
540 0.003
550 0.005
560 0.011
570 0.008
580 0.002
590 < 10⁻³
600 < 10⁻³
610 < 10⁻³
620 < 10⁻³
630 < 10⁻³
640 < 10⁻³
650 < 10⁻³
660 < 10⁻³
670 0.002
680 0.017
690 0.078
700 0.216
710 0.380
720 0.518
730 0.623
740 0.704
750 0.769
760 0.822
770 0.863
780 0.896
790 0.921
λ [nm]
800 0.939
810 0.952
820 0.961
830 0.967
840 0.972
850 0.974
860 0.976
870 0.976
880 0.977
890 0.976
900 0.975
910 0.974
920 0.973
930 0.971
940 0.968
950 0.965
960 0.962
970 0.957
980 0.952
990 0.946
1,000 0.938
1,010 0.929
1,020 0.918
1,030 0.905
1,040 0.890
1,050 0.872
1,060 0.851
1,070 0.827
1,080 0.801
1,090 0.771
λ [nm]
1,100 0.740
1,110 0.706
1,120 0.669
1,130 0.632
1,140 0.593
1,150 0.555
1,160 0.515
1,170 0.477
1,180 0.440
1,190 0.405
1,200 0.374
1,250 0.261
1,300 0.229
1,350 0.255
1,400 0.264
1,450 0.224
1,500 0.195
1,550 0.201
1,600 0.232
1,650 0.251
1,700 0.245
1,750 0.240
1,800 0.256
1,850 0.302
1,900 0.369
1,950 0.444
2,000 0.511
2,050 0.563
2,100 0.606
2,150 0.642
λ [nm]
2,200 0.668
2,250 0.695
2,300 0.723
2,350 0.742
2,400 0.753
2,450 0.753
2,500 0.746
2,550 0.738
2,600 0.727
2,650 0.711
2,700 0.673
2,750 0.441
2,800 0.304
2,850 0.277
2,900 0.267
2,950 0.254
3,000 0.232
3,050 0.205
3,100 0.176
3,150 0.148
3,200 0.123
3,250 0.102
3,300 0.084
3,350 0.070
3,400 0.059
3,450 0.052
3,500 0.046
3,550 0.044
3,600 0.043
3,650 0.043
λ [nm]
3,700 0.044
3,750 0.046
3,800 0.049
3,850 0.053
3,900 0.058
3,950 0.062
4,000 0.063
4,050 0.059
4,100 0.051
4,150 0.041
4,200 0.031
4,250 0.022
4,300 0.015
4,350 0.009
4,400 0.005
4,450 0.002
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.921
Reference thickness
d [mm] 4
Spectral values guaranteed
τi (405nm) ≤ 0,002
Refractive Indices n
nF (486.1 nm) = 1.516
nh (404.7 nm) = 1.525
ng (435.8 nm) = 1.521
ns (852.1 nm) = 1.502
ne (546.1 nm) = 1.512
nd (587.6 nm) = 1.510
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 2.54
Bubble content
Bubble class
Transformation temperature
Tg [°C] 481
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 8.7
α20°C/300°C [10-6/K] 10
α20°C/200°C [10-6/K]