S8008G

S8008G
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
S8008G - S8008G
Thickness
1.0
Reflection factor
0.9115
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320
330
340
350
360
370
380
390
400
410 0.004
420 0.010
430 0.017
440 0.030
450 0.051
460 0.082
470 0.125
480 0.179
490 0.266
λ [nm]
500 0.345
510 0.376
520 0.370
530 0.358
540 0.533
550 0.546
560 0.479
570 0.183
580 0.083
590 0.052
600 0.112
610 0.113
620 0.093
630 0.069
640 0.059
650 0.050
660 0.045
670 0.044
680 0.044
690 0.039
700 0.043
710 0.047
720 0.052
730 0.052
740 0.024
750 0.028
760 0.054
770 0.071
780 0.075
790 0.061
λ [nm]
800 0.038
810 0.028
820 0.071
830 0.092
840 0.104
850 0.110
860 0.106
870 0.098
880 0.093
890 0.112
900 0.130
910 0.145
920 0.156
930 0.166
940 0.176
950 0.185
960 0.195
970 0.204
980 0.215
990 0.225
1,000 0.237
1,010 0.248
1,020 0.260
1,030 0.272
1,040 0.283
1,050 0.295
1,060 0.307
1,070 0.319
1,080 0.331
1,090 0.342
λ [nm]
1,100 0.353
1,110 0.365
1,120 0.378
1,130 0.389
1,140 0.402
1,150 0.414
1,160 0.426
1,170 0.438
1,180 0.449
1,190 0.462
1,200 0.472
1,250 0.529
1,300 0.581
1,350 0.628
1,400 0.670
1,450 0.707
1,500 0.735
1,550 0.752
1,600 0.776
1,650 0.810
1,700 0.831
1,750 0.853
1,800 0.872
1,850 0.887
1,900 0.898
1,950 0.908
2,000 0.917
2,050 0.925
2,100 0.930
2,150 0.933
λ [nm]
2,200 0.930
2,250 0.929
2,300 0.905
2,350 0.836
2,400 0.804
2,450 0.821
2,500 0.834
2,550 0.855
2,600 0.878
2,650 0.899
2,700 0.894
2,750 0.625
2,800 0.494
2,850 0.501
2,900 0.520
2,950 0.539
3,000 0.554
3,050 0.563
3,100 0.566
3,150 0.562
3,200 0.555
3,250 0.545
3,300 0.535
3,350 0.524
3,400 0.514
3,450 0.505
3,500 0.500
3,550 0.499
3,600 0.502
3,650 0.506
λ [nm]
3,700 0.512
3,750 0.519
3,800 0.529
3,850 0.541
3,900 0.547
3,950 0.548
4,000 0.541
4,050 0.529
4,100 0.510
4,150 0.485
4,200 0.453
4,250 0.415
4,300 0.373
4,350 0.328
4,400 0.278
4,450 0.226
4,500 0.175
4,550 0.129
4,600 0.092
4,650 0.063
4,700 0.043
4,750 0.029
4,800 0.021
4,850 0.015
4,900 0.011
4,950 0.007
5,000 0.004
5,050 0.002
5,100 0.001
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.912
Reference thickness
d [mm] 1
Refractive Indices n
nF (486.1 nm) = 1.556
nh (404.7 nm) = 1.566
ng (435.8 nm) = 1.561
ns (852.1 nm) = 1.540
ne (546.1 nm) = 1.551
nd (587.6 nm) = 1.548
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 2.775
Bubble content
Bubble class
Transformation temperature
Tg [°C] 480
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.61
α20°C/300°C [10-6/K] 8.96
α20°C/200°C [10-6/K]