S8802

S8802
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
S8802 - S8802
Thickness
3.5
Reflection factor
0.9152
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290
300
310
320
330
340
350
360 0.003
370 0.115
380 0.136
390 0.320
400 0.468
410 0.456
420 0.386
430 0.244
440 0.178
450 0.206
460 0.216
470 0.185
480 0.180
490 0.286
λ [nm]
500 0.290
510 0.219
520 0.235
530 0.128
540 0.278
550 0.351
560 0.334
570 0.016
580 0.025
590 0.014
600 0.126
610 0.204
620 0.331
630 0.307
640 0.310
650 0.320
660 0.344
670 0.363
680 0.385
690 0.435
700 0.497
710 0.500
720 0.476
730 0.377
740 0.046
750 0.088
760 0.262
770 0.318
780 0.288
790 0.160
λ [nm]
800 0.059
810 0.029
820 0.151
830 0.226
840 0.256
850 0.250
860 0.206
870 0.156
880 0.134
890 0.155
900 0.180
910 0.189
920 0.190
930 0.187
940 0.182
950 0.177
960 0.171
970 0.166
980 0.162
990 0.157
1,000 0.153
1,010 0.150
1,020 0.148
1,030 0.145
1,040 0.143
1,050 0.141
1,060 0.139
1,070 0.137
1,080 0.136
1,090 0.135
λ [nm]
1,100 0.134
1,110 0.133
1,120 0.133
1,130 0.133
1,140 0.133
1,150 0.134
1,160 0.135
1,170 0.136
1,180 0.137
1,190 0.139
1,200 0.141
1,250 0.151
1,300 0.161
1,350 0.166
1,400 0.162
1,450 0.137
1,500 0.140
1,550 0.198
1,600 0.267
1,650 0.326
1,700 0.347
1,750 0.335
1,800 0.255
1,850 0.194
1,900 0.212
1,950 0.243
2,000 0.278
2,050 0.303
2,100 0.322
2,150 0.337
λ [nm]
2,200 0.343
2,250 0.342
2,300 0.330
2,350 0.283
2,400 0.286
2,450 0.318
2,500 0.340
2,550 0.351
2,600 0.358
2,650 0.371
2,700 0.365
2,750 0.253
2,800 0.158
2,850 0.136
2,900 0.130
2,950 0.126
3,000 0.119
3,050 0.108
3,100 0.094
3,150 0.079
3,200 0.066
3,250 0.055
3,300 0.046
3,350 0.039
3,400 0.033
3,450 0.029
3,500 0.026
3,550 0.025
3,600 0.026
3,650 0.027
λ [nm]
3,700 0.029
3,750 0.032
3,800 0.035
3,850 0.039
3,900 0.044
3,950 0.047
4,000 0.048
4,050 0.045
4,100 0.039
4,150 0.032
4,200 0.025
4,250 0.019
4,300 0.014
4,350 0.009
4,400 0.005
4,450 0.003
4,500 0.001
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750
4,800
4,850
4,900
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.915
Reference thickness
d [mm] 4
Refractive Indices n
nd (587.6 nm) = 1.533
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 2.7
Bubble content
Bubble class
Transformation temperature
Tg [°C] 510
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K]
α20°C/300°C [10-6/K] 10.8
α20°C/200°C [10-6/K]