S8806A

S8806A
Spectral values guaranteed
τi (550nm) >0.76
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
S8806A - S8806A
Thickness
2.5
Reflection factor
0.8780
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260
270
280
290 < 10⁻³
300 0.011
310 0.120
320 0.286
330 0.112
340 0.324
350 0.001
360 0.006
370 0.901
380 0.918
390 0.957
400 0.957
410 0.968
420 0.880
430 0.309
440 0.837
450 0.725
460 0.373
470 0.320
480 0.388
490 0.798
λ [nm]
500 0.376
510 0.027
520 0.026
530 0.011
540 0.454
550 0.805
560 0.693
570 0.002
580
590
600 0.051
610 0.735
620 0.833
630 0.760
640 0.906
650 0.973
660 0.954
670 0.675
680 0.325
690 0.534
700 0.833
710 0.897
720 0.739
730 0.072
740
750
760 0.010
770 0.272
780 0.227
790 0.005
λ [nm]
800
810
820 0.021
830 0.266
840 0.680
850 0.707
860 0.230
870 0.076
880 0.083
890 0.210
900 0.411
910 0.633
920 0.820
930 0.934
940 0.981
950 0.993
960 0.996
970 0.996
980 0.996
990 0.995
1,000 0.995
1,010 0.995
1,020 0.996
1,030 0.996
1,040 0.996
1,050 0.995
1,060 0.993
1,070 0.990
1,080 0.990
1,090 0.993
λ [nm]
1,100 0.996
1,110 0.997
1,120 0.998
1,130 0.999
1,140 0.999
1,150 1.000
1,160 1.000
1,170 0.999
1,180 0.999
1,190 0.997
1,200 0.994
1,250 0.992
1,300 0.996
1,350 0.980
1,400 0.944
1,450 0.923
1,500 0.847
1,550 0.727
1,600 0.678
1,650 0.723
1,700 0.776
1,750 0.862
1,800 0.938
1,850 0.941
1,900 0.925
1,950 0.930
2,000 0.940
2,050 0.943
2,100 0.935
2,150 0.911
λ [nm]
2,200 0.856
2,250 0.693
2,300 0.351
2,350 0.135
2,400 0.079
2,450 0.074
2,500 0.093
2,550 0.117
2,600 0.264
2,650 0.355
2,700 0.438
2,750 0.403
2,800 0.273
2,850 0.233
2,900 0.236
2,950 0.250
3,000 0.263
3,050 0.271
3,100 0.274
3,150 0.268
3,200 0.251
3,250 0.211
3,300 0.141
3,350 0.067
3,400 0.021
3,450 0.004
3,500 < 10⁻³
3,550
3,600
3,650
λ [nm]
3,700
3,750
3,800
3,850 < 10⁻³
3,900 < 10⁻³
3,950 < 10⁻³
4,000 < 10⁻³
4,050 < 10⁻³
4,100 < 10⁻³
4,150 < 10⁻³
4,200
4,250
4,300 < 10⁻³
4,350 < 10⁻³
4,400 < 10⁻³
4,450 < 10⁻³
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050
5,100
5,150
Optical values
Reflection factor
Pd 0.878
Reference thickness
d [mm] 2
Spectral values guaranteed
τi (550nm) >0.76
Refractive Indices n
nF (486.1 nm) = 1.694
nh (404.7 nm) = 1.707
ng (435.8 nm) = 1.701
ns (852.1 nm) = 1.674
ne (546.1 nm) = 1.688
nd (587.6 nm) = 1.685
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 3.4874
Bubble content
Bubble class -
Transformation temperature
Tg [°C] 653
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 4
SR class 52.0
AR class 1.3
Thermal expansion
α-30°C/+70°C [10-6/K] 6.13
α20°C/300°C [10-6/K] 7.27
α20°C/200°C [10-6/K]