技术规格
内部透过率(图表)
- SCHOTT
- S8023 - S8023
- 厚度
- 3.0
- 反射系数
- 0.9133
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | |
| 300 | |
| 310 | |
| 320 | < 10⁻³ |
| 330 | < 10⁻³ |
| 340 | < 10⁻³ |
| 350 | < 10⁻³ |
| 360 | 0.012 |
| 370 | 0.064 |
| 380 | 0.140 |
| 390 | 0.210 |
| 400 | 0.259 |
| 410 | 0.288 |
| 420 | 0.304 |
| 430 | 0.314 |
| 440 | 0.325 |
| 450 | 0.343 |
| 460 | 0.372 |
| 470 | 0.410 |
| 480 | 0.461 |
| 490 | 0.521 |
| λ [nm] | |
|---|---|
| 500 | 0.580 |
| 510 | 0.619 |
| 520 | 0.622 |
| 530 | 0.575 |
| 540 | 0.480 |
| 550 | 0.365 |
| 560 | 0.239 |
| 570 | 0.132 |
| 580 | 0.059 |
| 590 | 0.021 |
| 600 | 0.006 |
| 610 | 0.001 |
| 620 | < 10⁻³ |
| 630 | < 10⁻³ |
| 640 | < 10⁻³ |
| 650 | < 10⁻³ |
| 660 | < 10⁻³ |
| 670 | < 10⁻³ |
| 680 | < 10⁻³ |
| 690 | < 10⁻³ |
| 700 | < 10⁻³ |
| 710 | < 10⁻³ |
| 720 | < 10⁻³ |
| 730 | < 10⁻³ |
| 740 | < 10⁻³ |
| 750 | < 10⁻³ |
| 760 | < 10⁻³ |
| 770 | < 10⁻³ |
| 780 | < 10⁻³ |
| 790 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 800 | < 10⁻³ |
| 810 | < 10⁻³ |
| 820 | < 10⁻³ |
| 830 | < 10⁻³ |
| 840 | < 10⁻³ |
| 850 | < 10⁻³ |
| 860 | < 10⁻³ |
| 870 | < 10⁻³ |
| 880 | < 10⁻³ |
| 890 | < 10⁻³ |
| 900 | < 10⁻³ |
| 910 | < 10⁻³ |
| 920 | < 10⁻³ |
| 930 | < 10⁻³ |
| 940 | < 10⁻³ |
| 950 | < 10⁻³ |
| 960 | < 10⁻³ |
| 970 | < 10⁻³ |
| 980 | < 10⁻³ |
| 990 | < 10⁻³ |
| 1,000 | < 10⁻³ |
| 1,010 | < 10⁻³ |
| 1,020 | < 10⁻³ |
| 1,030 | < 10⁻³ |
| 1,040 | < 10⁻³ |
| 1,050 | < 10⁻³ |
| 1,060 | < 10⁻³ |
| 1,070 | < 10⁻³ |
| 1,080 | < 10⁻³ |
| 1,090 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 1,100 | < 10⁻³ |
| 1,110 | < 10⁻³ |
| 1,120 | < 10⁻³ |
| 1,130 | < 10⁻³ |
| 1,140 | < 10⁻³ |
| 1,150 | < 10⁻³ |
| 1,160 | < 10⁻³ |
| 1,170 | < 10⁻³ |
| 1,180 | < 10⁻³ |
| 1,190 | < 10⁻³ |
| 1,200 | < 10⁻³ |
| 1,250 | < 10⁻³ |
| 1,300 | < 10⁻³ |
| 1,350 | < 10⁻³ |
| 1,400 | < 10⁻³ |
| 1,450 | < 10⁻³ |
| 1,500 | < 10⁻³ |
| 1,550 | < 10⁻³ |
| 1,600 | < 10⁻³ |
| 1,650 | 0.001 |
| 1,700 | 0.004 |
| 1,750 | 0.011 |
| 1,800 | 0.024 |
| 1,850 | 0.044 |
| 1,900 | 0.072 |
| 1,950 | 0.107 |
| 2,000 | 0.149 |
| 2,050 | 0.195 |
| 2,100 | 0.243 |
| 2,150 | 0.291 |
| λ [nm] | |
|---|---|
| 2,200 | 0.332 |
| 2,250 | 0.373 |
| 2,300 | 0.414 |
| 2,350 | 0.453 |
| 2,400 | 0.489 |
| 2,450 | 0.519 |
| 2,500 | 0.537 |
| 2,550 | 0.545 |
| 2,600 | 0.550 |
| 2,650 | 0.555 |
| 2,700 | 0.548 |
| 2,750 | 0.499 |
| 2,800 | 0.269 |
| 2,850 | 0.112 |
| 2,900 | 0.059 |
| 2,950 | 0.037 |
| 3,000 | 0.026 |
| 3,050 | 0.018 |
| 3,100 | 0.013 |
| 3,150 | 0.010 |
| 3,200 | 0.007 |
| 3,250 | 0.006 |
| 3,300 | 0.005 |
| 3,350 | 0.004 |
| 3,400 | 0.004 |
| 3,450 | 0.004 |
| 3,500 | 0.005 |
| 3,550 | 0.005 |
| 3,600 | 0.006 |
| 3,650 | 0.008 |
| λ [nm] | |
|---|---|
| 3,700 | 0.009 |
| 3,750 | 0.008 |
| 3,800 | 0.005 |
| 3,850 | 0.003 |
| 3,900 | 0.001 |
| 3,950 | < 10⁻³ |
| 4,000 | < 10⁻³ |
| 4,050 | < 10⁻³ |
| 4,100 | < 10⁻³ |
| 4,150 | < 10⁻³ |
| 4,200 | < 10⁻³ |
| 4,250 | < 10⁻³ |
| 4,300 | < 10⁻³ |
| 4,350 | < 10⁻³ |
| 4,400 | < 10⁻³ |
| 4,450 | < 10⁻³ |
| 4,500 | < 10⁻³ |
| 4,550 | < 10⁻³ |
| 4,600 | < 10⁻³ |
| 4,650 | < 10⁻³ |
| 4,700 | < 10⁻³ |
| 4,750 | < 10⁻³ |
| 4,800 | < 10⁻³ |
| 4,850 | < 10⁻³ |
| 4,900 | < 10⁻³ |
| 4,950 | < 10⁻³ |
| 5,000 | < 10⁻³ |
| 5,050 | < 10⁻³ |
| 5,100 | < 10⁻³ |
| 5,150 | < 10⁻³ |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.913 |
| 参考厚度 | |
|---|---|
| d [mm] | 3 |
| 折射率 n |
|---|
| nF (486.1 nm) = 1.548 |
| nh (404.7 nm) = 1.568 |
| ng (435.8 nm) = 1.556 |
| ns (852.1 nm) = 1.537 |
| ne (546.1 nm) = 1.544 |
| nd (587.6 nm) = |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.277 | 0.218 | 0.189 |
| y | 0.459 | 0.474 | 0.486 |
| Y | 41 | 27 | 19 |
| λd [nm] | 500 | 500 | 500 |
| Pe | 0.39 | 0.52 | 0.59 |
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.262 | 0.209 | 0.182 |
| y | 0.437 | 0.449 | 0.460 |
| Y | 43 | 28 | 21 |
| λd [nm] | 498 | 498 | 499 |
| Pe | 0.39 | 0.52 | 0.59 |
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.206 | 0.176 | 0.160 |
| y | 0.328 | 0.334 | 0.346 |
| Y | 51 | 35 | 26 |
| λd [nm] | 491 | 492 | 493 |
| Pe | 0.39 | 0.50 | 0.54 |
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.75 |
| 气泡含量 | |
|---|---|
| 气泡等级 | |
| 玻转温度 | |
|---|---|
| Tg [°C] | 444 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | 0 |
| 耐酸性 | 4.0 |
| 耐碱性 | 3.0 |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | |
| α20°C/300°C [10-6/K] | |
| α20°C/200°C [10-6/K] | 9.7 |