N-SF6HT

Glass Code:  805254.337

"N"型环保玻璃替代传统的含铅和 砷的玻璃类型。

高透过率玻璃和超高透过率玻璃 - 透射性能更优,尤其是在蓝紫光谱范围内。

在下面的标签或我们的 网页上查找更多的信息。

我们目前可用的玻璃系列采用阿贝图表示, : 交互式阿贝图作为主要工具帮助您选择最合适玻璃。

optical glass klein 4zu3.jpg
Characteristics
nd 1.80518 νd 25.36
ne 1.81266 νe 25.16
nF-nC 0.031750 nF'-nC' 0.032304
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Refractive Indices
Characteristics λ [nm]
n2,325.4 2,325.4 1.74895
n1,970.1 1,970.1 1.75541
n1,529.6 1,529.6 1.76307
n1,060.0 1,060.0 1.77341
nt 1,014.0 1.77486
ns 852.1 1.78144
nr 706.5 1.79114
nC 656.3 1.79608
nC' 643.8 1.79749
Characteristics λ [nm]
n632.8 632.8 1.79883
nD 589.3 1.80491
nd 587.6 1.80518
ne 546.1 1.81266
nF 486.1 1.82783
nF' 480.0 1.82980
ng 435.8 1.84738
nh 404.7 1.86506
ni 365.0
Characteristics λ [nm]
n334.1 334.1
n312.6 312.6
n296.7 296.7
n280.4 280.4
n248.3 248.3
Internal Transmittance
Characteristics λ [nm]
τ25/2500 2,500 0.560
τ25/2325 2,325 0.620
τ25/1970 1,970 0.870
τ25/1530 1,530 0.980
τ25/1060 1,060 0.997
τ25/700 700 0.984
τ25/660 660 0.977
τ25/620 620 0.979
τ25/580 580 0.981
τ25/546 546 0.975
τ25/500 500 0.950
τ25/460 460 0.917
τ25/436 436 0.890
τ25/420 420 0.850
τ25/405 405 0.770
τ25/400 400 0.720
τ25/390 390 0.560
τ25/380 380 0.270
τ25/370 370 0.020
τ25/365 365
τ25/350 350
τ25/334 334
τ25/320 320
τ25/310 310
τ25/300 300
τ25/290 290
τ25/280 280
τ25/270 270
τ25/260 260
τ25/250 250
Characteristics λ [nm]
τ10/2500 2,500 0.793
τ10/2325 2,325 0.826
τ10/1970 1,970 0.946
τ10/1530 1,530 0.992
τ10/1060 1,060 0.999
τ10/700 700 0.994
τ10/660 660 0.991
τ10/620 620 0.992
τ10/580 580 0.992
τ10/546 546 0.990
τ10/500 500 0.980
τ10/460 460 0.966
τ10/436 436 0.954
τ10/420 420 0.937
τ10/405 405 0.901
τ10/400 400 0.877
τ10/390 390 0.793
τ10/380 380 0.592
τ10/370 370 0.209
τ10/365 365 0.004
τ10/350 350
τ10/334 334
τ10/320 320
τ10/310 310
τ10/300 300
τ10/290 290
τ10/280 280
τ10/270 270
τ10/260 260
τ10/250 250
Partial Dispersion
Characteristics
Ps,t 0.2074
PC,s 0.4610
Pd,C 0.2867
Pe,d 0.2356
Pg,F 0.6158
Pi,h
P's,t 0.2039
P'C',s 0.4969
P'd,C' 0.2380
P'e,d 0.2315
P'g,F' 0.5443
P'i,h
Characteristics
ΔPC,t 0.0031
ΔPC,s -0.0010
ΔPF,e 0.0027
ΔPg,F 0.0146
ΔPi,g