技术规格
内部透过率(图表)
- SCHOTT
- BG46 - BG46
- 厚度
- 1.0
- 反射系数
- 0.9100
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | |
| 300 | < 10⁻³ |
| 310 | < 10⁻³ |
| 320 | 0.002 |
| 330 | 0.049 |
| 340 | 0.181 |
| 350 | 0.323 |
| 360 | 0.428 |
| 370 | 0.503 |
| 380 | 0.563 |
| 390 | 0.614 |
| 400 | 0.650 |
| 410 | 0.683 |
| 420 | 0.707 |
| 430 | 0.731 |
| 440 | 0.752 |
| 450 | 0.771 |
| 460 | 0.795 |
| 470 | 0.816 |
| 480 | 0.842 |
| 490 | 0.866 |
| λ [nm] | |
|---|---|
| 500 | 0.889 |
| 510 | 0.902 |
| 520 | 0.908 |
| 530 | 0.895 |
| 540 | 0.862 |
| 550 | 0.807 |
| 560 | 0.727 |
| 570 | 0.621 |
| 580 | 0.501 |
| 590 | 0.373 |
| 600 | 0.258 |
| 610 | 0.161 |
| 620 | 0.091 |
| 630 | 0.047 |
| 640 | 0.021 |
| 650 | 0.009 |
| 660 | 0.003 |
| 670 | 0.001 |
| 680 | < 10⁻³ |
| 690 | < 10⁻³ |
| 700 | < 10⁻³ |
| 710 | < 10⁻³ |
| 720 | < 10⁻³ |
| 730 | < 10⁻³ |
| 740 | < 10⁻³ |
| 750 | < 10⁻³ |
| 760 | < 10⁻³ |
| 770 | < 10⁻³ |
| 780 | < 10⁻³ |
| 790 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 800 | < 10⁻³ |
| 810 | < 10⁻³ |
| 820 | < 10⁻³ |
| 830 | < 10⁻³ |
| 840 | < 10⁻³ |
| 850 | < 10⁻³ |
| 860 | < 10⁻³ |
| 870 | < 10⁻³ |
| 880 | < 10⁻³ |
| 890 | < 10⁻³ |
| 900 | < 10⁻³ |
| 910 | < 10⁻³ |
| 920 | < 10⁻³ |
| 930 | < 10⁻³ |
| 940 | < 10⁻³ |
| 950 | < 10⁻³ |
| 960 | < 10⁻³ |
| 970 | < 10⁻³ |
| 980 | < 10⁻³ |
| 990 | < 10⁻³ |
| 1,000 | < 10⁻³ |
| 1,010 | < 10⁻³ |
| 1,020 | < 10⁻³ |
| 1,030 | < 10⁻³ |
| 1,040 | < 10⁻³ |
| 1,050 | < 10⁻³ |
| 1,060 | < 10⁻³ |
| 1,070 | < 10⁻³ |
| 1,080 | < 10⁻³ |
| 1,090 | < 10⁻³ |
| λ [nm] | |
|---|---|
| 1,100 | < 10⁻³ |
| 1,110 | < 10⁻³ |
| 1,120 | < 10⁻³ |
| 1,130 | < 10⁻³ |
| 1,140 | < 10⁻³ |
| 1,150 | < 10⁻³ |
| 1,160 | < 10⁻³ |
| 1,170 | < 10⁻³ |
| 1,180 | < 10⁻³ |
| 1,190 | < 10⁻³ |
| 1,200 | < 10⁻³ |
| 1,250 | < 10⁻³ |
| 1,300 | < 10⁻³ |
| 1,350 | < 10⁻³ |
| 1,400 | 0.003 |
| 1,450 | 0.008 |
| 1,500 | 0.021 |
| 1,550 | 0.045 |
| 1,600 | 0.082 |
| 1,650 | 0.133 |
| 1,700 | 0.198 |
| 1,750 | 0.272 |
| 1,800 | 0.349 |
| 1,850 | 0.426 |
| 1,900 | 0.499 |
| 1,950 | 0.566 |
| 2,000 | 0.625 |
| 2,050 | 0.676 |
| 2,100 | 0.720 |
| 2,150 | 0.756 |
| λ [nm] | |
|---|---|
| 2,200 | 0.776 |
| 2,250 | 0.794 |
| 2,300 | 0.814 |
| 2,350 | 0.834 |
| 2,400 | 0.849 |
| 2,450 | 0.859 |
| 2,500 | 0.858 |
| 2,550 | 0.845 |
| 2,600 | 0.828 |
| 2,650 | 0.822 |
| 2,700 | 0.804 |
| 2,750 | 0.742 |
| 2,800 | 0.454 |
| 2,850 | 0.240 |
| 2,900 | 0.149 |
| 2,950 | 0.104 |
| 3,000 | 0.078 |
| 3,050 | 0.061 |
| 3,100 | 0.050 |
| 3,150 | 0.042 |
| 3,200 | 0.037 |
| 3,250 | 0.033 |
| 3,300 | 0.032 |
| 3,350 | 0.032 |
| 3,400 | 0.034 |
| 3,450 | 0.037 |
| 3,500 | 0.041 |
| 3,550 | 0.048 |
| 3,600 | 0.056 |
| 3,650 | 0.064 |
| λ [nm] | |
|---|---|
| 3,700 | 0.069 |
| 3,750 | 0.067 |
| 3,800 | 0.057 |
| 3,850 | 0.046 |
| 3,900 | 0.033 |
| 3,950 | 0.020 |
| 4,000 | 0.012 |
| 4,050 | 0.008 |
| 4,100 | 0.005 |
| 4,150 | 0.003 |
| 4,200 | 0.003 |
| 4,250 | 0.002 |
| 4,300 | 0.003 |
| 4,350 | 0.005 |
| 4,400 | 0.008 |
| 4,450 | 0.011 |
| 4,500 | 0.013 |
| 4,550 | 0.016 |
| 4,600 | 0.020 |
| 4,650 | 0.025 |
| 4,700 | 0.031 |
| 4,750 | 0.037 |
| 4,800 | 0.042 |
| 4,850 | 0.047 |
| 4,900 | 0.050 |
| 4,950 | 0.051 |
| 5,000 | 0.048 |
| 5,050 | 0.040 |
| 5,100 | 0.029 |
| 5,150 | 0.017 |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.910 |
| 参考厚度 | |
|---|---|
| d [mm] | 1 |
| 承诺光谱值 | |
|---|---|
| τi (514nm) | ≥ 0,89 |
| τi (700nm) | ≤ 0,0001 |
| 折射率 n |
|---|
| nF (486.1 nm) = 1.561 |
| nh (404.7 nm) = 1.573 |
| ng (435.8 nm) = 1.567 |
| ns (852.1 nm) = 1.547 |
| ne (546.1 nm) = 1.557 |
| nd (587.6 nm) = 1.554 |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.302 | 0.246 | 0.216 |
| y | 0.457 | 0.475 | 0.487 |
| Y | 49 | 35 | 27 |
| λd [nm] | 501 | 501 | 501 |
| Pe | 0.33 | 0.46 | 0.53 |
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.285 | 0.234 | 0.207 |
| y | 0.438 | 0.452 | 0.463 |
| Y | 51 | 37 | 29 |
| λd [nm] | 499 | 499 | 499 |
| Pe | 0.33 | 0.46 | 0.52 |
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.221 | 0.191 | 0.175 |
| y | 0.333 | 0.340 | 0.351 |
| Y | 58 | 45 | 36 |
| λd [nm] | 492 | 493 | 493 |
| Pe | 0.33 | 0.44 | 0.49 |
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.7917 |
| 气泡含量 | |
|---|---|
| 气泡等级 | |
| 玻转温度 | |
|---|---|
| Tg [°C] | 386 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | 0 |
| 耐酸性 | 4.0 |
| 耐碱性 | 4.3 |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | 8.09 |
| α20°C/300°C [10-6/K] | 9.98 |
| α20°C/200°C [10-6/K] | |