技术规格
内部透过率(图表)
- SCHOTT
- S7000 - S7000
- 厚度
- 2.0
- 反射系数
- 0.9080
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | < 10⁻³ |
| 210 | < 10⁻³ |
| 220 | < 10⁻³ |
| 230 | < 10⁻³ |
| 240 | < 10⁻³ |
| 250 | < 10⁻³ |
| 260 | < 10⁻³ |
| 270 | < 10⁻³ |
| 280 | 0.004 |
| 290 | 0.015 |
| 300 | 0.022 |
| 310 | 0.021 |
| 320 | 0.038 |
| 330 | 0.154 |
| 340 | 0.462 |
| 350 | 0.755 |
| 360 | 0.896 |
| 370 | 0.951 |
| 380 | 0.972 |
| 390 | 0.981 |
| 400 | 0.987 |
| 410 | 0.991 |
| 420 | 0.993 |
| 430 | 0.993 |
| 440 | 0.995 |
| 450 | 0.995 |
| 460 | 0.995 |
| 470 | 0.997 |
| 480 | 0.998 |
| 490 | 0.997 |
| λ [nm] | |
|---|---|
| 500 | 0.996 |
| 510 | 0.997 |
| 520 | 0.998 |
| 530 | 0.998 |
| 540 | 0.999 |
| 550 | 0.999 |
| 560 | 0.992 |
| 570 | 1.000 |
| 580 | 1.000 |
| 590 | 1.000 |
| 600 | 0.992 |
| 610 | 0.992 |
| 620 | 0.992 |
| 630 | 0.992 |
| 640 | 0.992 |
| 650 | 0.993 |
| 660 | 0.993 |
| 670 | 0.993 |
| 680 | 0.993 |
| 690 | 0.993 |
| 700 | 0.993 |
| 710 | 0.992 |
| 720 | 0.993 |
| 730 | 0.994 |
| 740 | 0.993 |
| 750 | 0.994 |
| 760 | 0.992 |
| 770 | 0.995 |
| 780 | 0.993 |
| 790 | 0.993 |
| λ [nm] | |
|---|---|
| 800 | 0.994 |
| 810 | 0.996 |
| 820 | 0.994 |
| 830 | 0.995 |
| 840 | 0.996 |
| 850 | 0.994 |
| 860 | 0.994 |
| 870 | 0.996 |
| 880 | 0.997 |
| 890 | 0.996 |
| 900 | 0.997 |
| 910 | 0.997 |
| 920 | 0.997 |
| 930 | 0.997 |
| 940 | 0.997 |
| 950 | 0.997 |
| 960 | 0.997 |
| 970 | 0.997 |
| 980 | 0.997 |
| 990 | 0.997 |
| 1,000 | 0.997 |
| 1,010 | 0.997 |
| 1,020 | 0.997 |
| 1,030 | 0.997 |
| 1,040 | 0.997 |
| 1,050 | 0.997 |
| 1,060 | 0.997 |
| 1,070 | 0.997 |
| 1,080 | 0.997 |
| 1,090 | 0.997 |
| λ [nm] | |
|---|---|
| 1,100 | 0.997 |
| 1,110 | 0.997 |
| 1,120 | 0.997 |
| 1,130 | 0.998 |
| 1,140 | 0.997 |
| 1,150 | 0.997 |
| 1,160 | 0.998 |
| 1,170 | 0.998 |
| 1,180 | 0.997 |
| 1,190 | 0.998 |
| 1,200 | 0.998 |
| 1,250 | 0.998 |
| 1,300 | 0.998 |
| 1,350 | 0.999 |
| 1,400 | 0.998 |
| 1,450 | 0.998 |
| 1,500 | 0.998 |
| 1,550 | 0.998 |
| 1,600 | 0.998 |
| 1,650 | 0.998 |
| 1,700 | 0.998 |
| 1,750 | 0.998 |
| 1,800 | 0.998 |
| 1,850 | 0.997 |
| 1,900 | 0.997 |
| 1,950 | 0.997 |
| 2,000 | 0.998 |
| 2,050 | 0.998 |
| 2,100 | 0.996 |
| 2,150 | 0.995 |
| λ [nm] | |
|---|---|
| 2,200 | 0.995 |
| 2,250 | 0.992 |
| 2,300 | 0.992 |
| 2,350 | 0.992 |
| 2,400 | 1.000 |
| 2,450 | 0.998 |
| 2,500 | 0.994 |
| 2,550 | 0.993 |
| 2,600 | 0.992 |
| 2,650 | 0.990 |
| 2,700 | 0.981 |
| 2,750 | 0.871 |
| 2,800 | 0.765 |
| 2,850 | 0.751 |
| 2,900 | 0.748 |
| 2,950 | 0.747 |
| 3,000 | 0.747 |
| 3,050 | 0.743 |
| 3,100 | 0.735 |
| 3,150 | 0.725 |
| 3,200 | 0.712 |
| 3,250 | 0.698 |
| 3,300 | 0.683 |
| 3,350 | 0.665 |
| 3,400 | 0.643 |
| 3,450 | 0.619 |
| 3,500 | 0.595 |
| 3,550 | 0.580 |
| 3,600 | 0.572 |
| 3,650 | 0.562 |
| λ [nm] | |
|---|---|
| 3,700 | 0.549 |
| 3,750 | 0.529 |
| 3,800 | 0.522 |
| 3,850 | 0.533 |
| 3,900 | 0.540 |
| 3,950 | 0.535 |
| 4,000 | 0.516 |
| 4,050 | 0.495 |
| 4,100 | 0.480 |
| 4,150 | 0.465 |
| 4,200 | 0.445 |
| 4,250 | 0.415 |
| 4,300 | 0.368 |
| 4,350 | 0.310 |
| 4,400 | 0.242 |
| 4,450 | 0.172 |
| 4,500 | 0.110 |
| 4,550 | 0.061 |
| 4,600 | 0.030 |
| 4,650 | 0.014 |
| 4,700 | 0.006 |
| 4,750 | 0.003 |
| 4,800 | 0.001 |
| 4,850 | < 10⁻³ |
| 4,900 | < 10⁻³ |
| 4,950 | < 10⁻³ |
| 5,000 | < 10⁻³ |
| 5,050 | < 10⁻³ |
| 5,100 | < 10⁻³ |
| 5,150 | < 10⁻³ |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.908 |
| 参考厚度 | |
|---|---|
| d [mm] | 2 |
| 承诺光谱值 | |
|---|---|
| λs (τi = 0.00001) [nm] | 260 nm |
| λc (τi = 0.5) [nm] | 340 nm ± 6 nm |
| λp1 (τi = 0.99) [nm] | 420 nm |
| 折射率 n |
|---|
| nd (587.6 nm) = 1.563 |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.448 | 0.448 | 0.448 |
| y | 0.408 | 0.408 | 0.408 |
| Y | 91 | 91 | 91 |
| λd [nm] | 584 | 584 | 584 |
| Pe | 0.00 | 0.00 | 0.01 |
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.424 | 0.424 | 0.424 |
| y | 0.399 | 0.399 | 0.399 |
| Y | 91 | 91 | 91 |
| λd [nm] | 583 | 583 | 583 |
| Pe | 0.00 | 0.00 | 0.00 |
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.313 | 0.313 | 0.313 |
| y | 0.329 | 0.329 | 0.330 |
| Y | 91 | 91 | 91 |
| λd [nm] | 574 | 574 | 575 |
| Pe | 0.00 | 0.00 | 0.00 |
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.83 |
| 气泡含量 | |
|---|---|
| 气泡等级 | |
| 玻转温度 | |
|---|---|
| Tg [°C] | 452 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | 1.0 |
| 耐酸性 | 1.2 |
| 耐碱性 | 1.0 |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | 8.13 |
| α20°C/300°C [10-6/K] | 11.1 |
| α20°C/200°C [10-6/K] | |