技术规格
内部透过率(图表)
- SCHOTT
- S7005 - S7005
- 厚度
- 2.0
- 反射系数
- 0.9080
内部透过率(表格)
| λ [nm] | |
|---|---|
| 200 | |
| 210 | |
| 220 | |
| 230 | |
| 240 | |
| 250 | |
| 260 | |
| 270 | |
| 280 | |
| 290 | |
| 300 | |
| 310 | |
| 320 | |
| 330 | < 10⁻³ |
| 340 | 0.002 |
| 350 | 0.098 |
| 360 | 0.367 |
| 370 | 0.650 |
| 380 | 0.806 |
| 390 | 0.882 |
| 400 | 0.683 |
| 410 | 0.881 |
| 420 | 0.937 |
| 430 | 0.978 |
| 440 | 0.976 |
| 450 | 0.982 |
| 460 | 0.958 |
| 470 | 0.928 |
| 480 | 0.961 |
| 490 | 0.972 |
| λ [nm] | |
|---|---|
| 500 | 0.987 |
| 510 | 0.997 |
| 520 | 0.998 |
| 530 | 0.996 |
| 540 | 0.998 |
| 550 | 0.998 |
| 560 | 0.996 |
| 570 | 0.998 |
| 580 | 1.000 |
| 590 | 0.997 |
| 600 | 0.997 |
| 610 | 0.997 |
| 620 | 0.997 |
| 630 | 0.997 |
| 640 | 0.997 |
| 650 | 0.998 |
| 660 | 0.998 |
| 670 | 0.998 |
| 680 | 0.998 |
| 690 | 0.998 |
| 700 | 0.998 |
| 710 | 0.998 |
| 720 | 0.999 |
| 730 | 0.999 |
| 740 | 0.998 |
| 750 | 0.999 |
| 760 | 0.998 |
| 770 | 0.999 |
| 780 | 0.999 |
| 790 | 0.998 |
| λ [nm] | |
|---|---|
| 800 | 0.998 |
| 810 | 0.999 |
| 820 | 0.999 |
| 830 | 0.999 |
| 840 | 0.998 |
| 850 | 0.998 |
| 860 | 0.999 |
| 870 | 0.999 |
| 880 | 0.999 |
| 890 | 0.999 |
| 900 | 0.998 |
| 910 | 0.998 |
| 920 | 0.992 |
| 930 | 0.981 |
| 940 | 0.974 |
| 950 | 0.976 |
| 960 | 0.984 |
| 970 | 0.993 |
| 980 | 0.998 |
| 990 | 0.997 |
| 1,000 | 0.997 |
| 1,010 | 0.999 |
| 1,020 | 0.997 |
| 1,030 | 0.992 |
| 1,040 | 0.980 |
| 1,050 | 0.943 |
| 1,060 | 0.859 |
| 1,070 | 0.777 |
| 1,080 | 0.798 |
| 1,090 | 0.875 |
| λ [nm] | |
|---|---|
| 1,100 | 0.915 |
| 1,110 | 0.940 |
| 1,120 | 0.967 |
| 1,130 | 0.987 |
| 1,140 | 0.994 |
| 1,150 | 0.994 |
| 1,160 | 0.990 |
| 1,170 | 0.983 |
| 1,180 | 0.965 |
| 1,190 | 0.925 |
| 1,200 | 0.849 |
| 1,250 | 0.844 |
| 1,300 | 0.954 |
| 1,350 | 0.801 |
| 1,400 | 0.835 |
| 1,450 | 0.793 |
| 1,500 | 0.837 |
| 1,550 | 0.851 |
| 1,600 | 0.925 |
| 1,650 | 0.972 |
| 1,700 | 0.998 |
| 1,750 | 0.997 |
| 1,800 | 0.991 |
| 1,850 | 0.983 |
| 1,900 | 0.978 |
| 1,950 | 0.976 |
| 2,000 | 0.979 |
| 2,050 | 0.987 |
| 2,100 | 0.988 |
| 2,150 | 0.989 |
| λ [nm] | |
|---|---|
| 2,200 | 0.988 |
| 2,250 | 0.984 |
| 2,300 | 0.983 |
| 2,350 | 0.978 |
| 2,400 | 0.968 |
| 2,450 | 0.951 |
| 2,500 | 0.931 |
| 2,550 | 0.921 |
| 2,600 | 0.916 |
| 2,650 | 0.917 |
| 2,700 | 0.904 |
| 2,750 | 0.769 |
| 2,800 | 0.614 |
| 2,850 | 0.583 |
| 2,900 | 0.571 |
| 2,950 | 0.561 |
| 3,000 | 0.553 |
| 3,050 | 0.544 |
| 3,100 | 0.531 |
| 3,150 | 0.516 |
| 3,200 | 0.498 |
| 3,250 | 0.480 |
| 3,300 | 0.462 |
| 3,350 | 0.444 |
| 3,400 | 0.425 |
| 3,450 | 0.406 |
| 3,500 | 0.393 |
| 3,550 | 0.387 |
| 3,600 | 0.389 |
| 3,650 | 0.390 |
| λ [nm] | |
|---|---|
| 3,700 | 0.387 |
| 3,750 | 0.377 |
| 3,800 | 0.372 |
| 3,850 | 0.383 |
| 3,900 | 0.394 |
| 3,950 | 0.397 |
| 4,000 | 0.384 |
| 4,050 | 0.364 |
| 4,100 | 0.347 |
| 4,150 | 0.334 |
| 4,200 | 0.322 |
| 4,250 | 0.306 |
| 4,300 | 0.280 |
| 4,350 | 0.247 |
| 4,400 | 0.203 |
| 4,450 | 0.151 |
| 4,500 | 0.098 |
| 4,550 | 0.053 |
| 4,600 | 0.018 |
| 4,650 | 0.010 |
| 4,700 | 0.010 |
| 4,750 | 0.010 |
| 4,800 | 0.010 |
| 4,850 | 0.010 |
| 4,900 | 0.010 |
| 4,950 | 0.010 |
| 5,000 | 0.010 |
| 5,050 | 0.018 |
| 5,100 | 0.014 |
| 5,150 | 0.015 |
光学值
| 反射系数 | |
|---|---|
| Pd | 0.908 |
| 参考厚度 | |
|---|---|
| d [mm] | 2 |
| 承诺光谱值 | |
|---|---|
| λs (τi = 0.00001) [nm] | 330 |
| λc (τi = 0.5) [nm] | 365 ± 6 |
| 折射率 n |
|---|
| nd (587.6 nm) = 1.562 |
色度评估
| 光源 | A(Planck T = 2347K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.449 | 0.450 | 0.451 |
| y | 0.408 | 0.409 | 0.410 |
| Y | 91 | 91 | 90 |
| λd [nm] | 582 | 582 | 582 |
| Pe | 0.01 | 0.03 | 0.04 |
| 光源 | Planck T = 3200 K | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.425 | 0.426 | 0.427 |
| y | 0.400 | 0.401 | 0.402 |
| Y | 91 | 91 | 90 |
| λd [nm] | 580 | 580 | 580 |
| Pe | 0.01 | 0.03 | 0.04 |
| 光源 | D65 (TC = 6504 K) | ||
|---|---|---|---|
| d [mm] | 1 | 2 | 3 |
| x | 0.314 | 0.316 | 0.317 |
| y | 0.331 | 0.333 | 0.335 |
| Y | 91 | 90 | 90 |
| λd [nm] | 572 | 572 | 572 |
| Pe | 0.01 | 0.02 | 0.03 |
物理值
| 密度 | |
|---|---|
| p [g/cm3] | 2.88 |
| 气泡含量 | |
|---|---|
| 气泡等级 | - |
| 玻转温度 | |
|---|---|
| Tg [°C] | 452 |
| 温度系数 | |
|---|---|
| Tk [nm/°C] | |
| 耐化学性 | |
|---|---|
| 耐污性 | - |
| 耐酸性 | - |
| 耐碱性 | - |
| 热膨胀 | |
|---|---|
| α-30°C/+70°C [10-6/K] | |
| α20°C/300°C [10-6/K] | 11.5 |
| α20°C/200°C [10-6/K] | |